Anthracite-based graphite negative electrode material and preparation method thereof
Through the mechanical treatment of anthracite and the etching of sulfur to form a pore structure, combined with binder and mechanical granulation technology, the problem of fast charging and compaction density of artificial graphite anode materials has been solved, and efficient lithium-ion battery anode material performance and Simplify the process.
Patent Information
- Application Number
- CN202410848593.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The existing technology is difficult to effectively improve the fast charging and compaction density of artificial graphite anode materials, and the process is complex, which increases production costs.
Using anthracite as raw material, through mechanical crushing, flotation, gradient pre-carbonization and graphitization, combined with the etching of sulfur and the escape of minerals in the ash to form a pore structure, the binder and mechanical granulation technology are used to prepare high-quality Anthracite-based graphite anode material with compacted density and high discharge capacity.
The anthracite-based graphite anode material has high compaction density, large discharge capacity and good rate performance, simplifies the process steps, reduces production costs, and is suitable for industrial production.
Smart Images

Figure CN118851165A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery negative electrode materials, and specifically relates to an anthracite-based graphite negative electrode material and a preparation method thereof. Background Art
[0002] With the continuous development of economy and the acceleration of industrialization, the global energy demand has increased dramatically. The energy resource crisis and environmental problems make it urgent to develop clean, efficient and sustainable energy. Renewable energy such as wind power and solar energy are important driving forces for achieving sustainable development. In addition, the automotive industry, as one of the main sources of greenhouse gases in the world, has also become the focus of global attention. Therefore, electric vehicles (EV) and plug-in hybrid electric vehicles (PHEV) driven by lithium-ion batteries (LIB) have gradually become the focus of attention and are showing an explosive growth trend. The International Energy Agency (IEA) predicts that the global electric vehicle industry will grow significantly in the next decade, and the global electric vehicle ownership is expected to reach 230 million by 2030. Despite rapid progress in the long driving range and low cost of electric vehicles, consumers still lack acceptance of electric vehicles. This is mainly due to the long charging time of electric vehicles and the lingering range anxiety problem.
[0003] Graphite is the most thermodynamically stable carbon allotrope and is a successfully commercialized negative electrode material for lithium-ion batteries (LIBs). Graphite is composed of layered hexagonal carbon stacked by weak van der Waals interactions, in which sp2 hybridized carbon atoms are arranged in a hexagonal ring structure. There are two types of graphite negative electrode materials, namely natural graphite and artificial graphite. Among them, although natural graphite has a high specific capacity (>350mAh / g), its structure is unstable and easily causes the co-insertion of solvent molecules, resulting in the shedding of sheets during the charge and discharge process, causing poor battery cycle performance and safety. The core of the preparation process of artificial graphite is still the Acheson process, which is an energy-intensive process (about 3000℃). This process is heavily dependent on graphite precursors. So far, artificial graphite is mainly prepared using petroleum coke (including needle coke) and coal tar pitch as raw materials. However, these negative electrode materials, namely traditional graphite negative electrode materials, have small interlayer spacing and long migration paths. Under fast charging and high current, lithium is easily deposited on the graphite surface, forming lithium dendrites; not only does it reduce the battery capacity, it also punctures the diaphragm, causing a short circuit in the battery, leading to safety problems.
[0004] Anthracite is in the transition stage from coal to graphite. It has a similar molecular structure to petroleum coke, asphalt coke and other raw materials and can be converted into graphite at high temperatures. In particular, anthracite has a high carbon content (>93%) and moderate volatile matter (<10%). It has abundant pores inside and contains a certain graphite crystallite / microchip structure. The carbon atom layer has good preferential orientation in the short range and other characteristics. It can be converted into graphite at high temperatures with high yield and low price. It is an ideal material for preparing negative electrode materials for lithium-ion batteries.
[0005] Therefore, in order to overcome the problem of fast charging of graphite negative electrode materials, existing technologies include Chinese patent CN114094079B, which uses alkali metals such as KOH to etch and create pores in graphite sheets to enhance lithium ion transmission. However, this method requires the use of alkali metals, which has a great impact on production equipment, alkali metal processing, etc. Japanese patent JP2000243398 uses asphalt pyrolysis gas to treat the graphite surface, but the effect of improving the morphology of the material is limited, resulting in a low improvement in electrical performance. U.S. Patent US2006001003 introduces a catalyst, which improves the fast charging and discharging performance and cycle performance through catalyst intercalation and efficient graphitization; however, this method increases the process cost, and there are also engineering problems such as catalysts that are prone to cause spraying.
[0006] In view of this, the above-mentioned existing technologies are difficult to effectively improve the fast charging and compaction density problems of artificial graphite negative electrode materials. Summary of the invention
[0007] In view of the complex process problems such as special pore formation or small particle size and high energy consumption in the prior art, and the defects of poor fast charging performance and low compaction density of the prepared artificial graphite negative electrode material, the present invention provides an anthracite-based graphite negative electrode material and a preparation method thereof. The present invention controls the ash and sulfur content of anthracite within a certain range, and utilizes the etching of sulfur and the escape of minerals in the ash to form a pore structure in situ. The prepared anthracite-based graphite negative electrode material has high compaction density, large discharge capacity and good rate performance, and the process is simple, which has good compatibility with the current artificial graphite negative electrode process and is suitable for industrial production.
[0008] To achieve the above object, the technical solution of the present invention is as follows:
[0009] A first aspect of the present invention is a method for preparing an anthracite-based graphite negative electrode material, comprising the following steps:
[0010] Step 1: subjecting the anthracite to mechanical crushing, flotation, and mechanical pulverization in sequence and then to gradient pre-carbonization treatment to obtain pre-carbonized material;
[0011] Step 2: Graphitizing the pre-carbonized material to obtain anthracite-based artificial graphite primary particles.
[0012] Furthermore, the preparation method further comprises step 3: mixing the anthracite-based artificial graphite primary particles with a binder and then mechanically granulating them under heating conditions, and obtaining anthracite-based artificial graphite secondary particles by carbonization.
[0013] Preferably, the sulfur content of the anthracite is 1-3 wt %. The sulfur in the anthracite is preferably in the form of FeS 2 Mainly, FeS 2 The preferred proportion is ≥45%.
[0014] Preferably, the anthracite has a particle size D50 of 75-200 μm after mechanical crushing, an ash content of 2-5 wt% after flotation, and a particle size D50 of 5-10 μm after mechanical pulverization.
[0015] Preferably, the specific conditions of the gradient pre-carbonization treatment are: carried out under argon or helium, the final pre-carbonization temperature is 1050°C, and the gradient pre-carbonization curve is: the heating rate in the range of 0-600°C is 20-30°C / min, preferably 26-30°C / min, the heating rate in the range of 600-900°C is 10-18°C, preferably 10-15°C / min, and the heating rate in the range of 900-1100°C is 2-5°C / min, preferably 2-3°C / min.
[0016] Preferably, the specific conditions of the graphitization treatment are: the graphitization temperature is 2800-3200°C, the graphitization time is 16-32h, and the graphitization furnace is one of an induction vacuum graphitization furnace, an Acheson crucible furnace, an Acheson box furnace or an Acheson inner series furnace.
[0017] Preferably, the binder is one of oxidized asphalt, cross-linked asphalt, phenolic resin, epoxy resin, polyester resin, vinyl ester, bismaleamide, polyimide, and cyanate ester.
[0018] Preferably, the specific process of the mechanical granulation is: the anthracite-based artificial graphite primary particles and the binder are mixed at a mass ratio of (90-98): (2-10) at a high speed of 150-500 rpm at room temperature for 30-60 min, then the rotation speed is reduced to 20-100 rpm, and heated to 150-300°C for fusion granulation for 30-60 min; the specific conditions of the carbonization are: in a nitrogen atmosphere, the carbonization treatment is carried out at a heating rate of 5°C / min for 1-2 h, and the final carbonization temperature is 1200-1400°C.
[0019] The second aspect of the present invention is an anthracite-based graphite negative electrode material prepared by the preparation method of the first aspect, comprising anthracite-based artificial graphite primary particles with a particle size D50 of 5-10 μm and anthracite-based artificial graphite secondary particles with a particle size D50 of 11-20 μm. Its performance parameters are shown in Table 1.
[0020] Table 1
[0021] Serial number Projects and parameters index 1 Particle size (D50) 5-20μm 2 <![CDATA[True density (g / cm 3 )]]> ≥2.1 3 Ash content (wt%) ≤0.03 4 <![CDATA[Compaction density (g / cm 3 )]]> ≥1.75 5 <![CDATA[Specific surface area (m 2 / g)]]> ≤1.0-4.0 6 First discharge specific capacity (mAh / g) ≥345.0 7 First charge and discharge efficiency (%) ≥92.0 8 Rate performance (5C / 0.2C) ≥82.0
[0022] The third aspect of the present invention is a negative electrode material for a lithium-ion battery, comprising the anthracite-based graphite negative electrode material described in the second aspect.
[0023] A fourth aspect of the present invention is a lithium ion battery, comprising the lithium ion battery negative electrode material described in the third aspect.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The anthracite-based graphite negative electrode material prepared by the present invention has a reasonable pore structure, and these pore structures are not achieved by introducing an external activator, but by making full use of the structural characteristics of the coal itself to achieve in-situ pore formation. These pores come from two aspects. On the one hand, the FeS 2 Anthracite, which has the highest content in the form of existence, is used as the raw material. The sulfur contained in the coal is rapidly released in the form of gas under the action of thermochemistry to etch the coal surface to form pores. On the other hand, the volatile matter and minerals in ... the volatile matter in the volatile matter and minerals in the volatile matter and minerals in the volatile matter and the volatile matter in the volatile matter and minerals in the volatile matter and the volatile matter in the volatile matter and the minerals in the volatile matter and the volatile matter in the volatile matter and the minerals in the volatile matter and the volatile matter in
[0026] 2. Choose FeS 2 Anthracite with the highest content in the form of FeS is used as raw material. During the rapid heating process in the low temperature zone (0-600℃), FeS 2 It can be fully decomposed, and the S in it is converted into organic sulfur, which realizes the etching of coal in the thermochemical process of graphitization; while the Fe in it can undergo chemical reaction and act as an in-situ catalyst in the graphitization process to promote the graphitization process of coal.
[0027] 3. The gradient pre-carbonization technology is used to achieve effective regulation of the coal pore structure. The low temperature zone is mainly used to discharge moisture and low-temperature volatiles. At the same time, a fast heating rate is still used in the high temperature section to allow more cracking gases such as coal gas to escape. In the high temperature zone, a slow heating rate is used, which belongs to the condensation reaction temperature zone of coal molecules. On the one hand, it increases the pyrolysis time of coal in this temperature zone, and on the other hand, it strengthens the selectivity of the thermal reaction, so that it undergoes parallel and sequential pyrolysis reactions, thereby forming a certain stabilized orientation structure.
[0028] 4. The heated mechanical granulation process was introduced. Through the dual effects of the binder and mechanical extrusion, particles of different sizes were squeezed and adhered together, achieving effective fusion granulation of primary particles to form secondary particles, and improving the tap density and compaction density. The aggregation of primary particles provides a shorter lithium ion channel, thereby improving the rate performance.
[0029] 5. For the first time, a non-nitrogen inert atmosphere pre-carbonization technology was proposed, which avoided the participation of nitrogen in the thermal reaction during the pyrolysis process and reduced the sp2 carbon content.
[0030] 6. Through in-situ pore-making technology and heated mechanical granulation technology, the process steps are simplified and the production cost is reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a SEM image of the anthracite-based artificial graphite primary particles of the present invention.
[0032] Figure 2 This is the SEM image of the anthracite-based artificial graphite secondary particles of the present invention.
[0033] Figure 3 This is the SEM image of the comparative focal-based artificial graphite of the present invention.
[0034] Figure 4 This is the XRD diagram of the anthracite-based artificial graphite of the present invention.
[0035] Figure 5 This is a charge and discharge curve diagram of the anthracite-based artificial graphite of the present invention.
[0036] Figure 6 This is a graph showing the cycle performance (0.5C) of the anthracite-based artificial graphite of the present invention. DETAILED DESCRIPTION
[0037] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0038] Example 1
[0039] Anthracite (sulfur content of 1.5wt%) was crushed to a particle size of 75μm by mechanical crushing, and then the ash content was reduced to 2.5wt% by flotation. Then, the particle size was reduced to 10μm by a mechanical crusher, and then pre-carbonized by a gradient pre-carbonization program in a helium atmosphere, with a final pre-carbonization temperature of 1050°C to obtain a pre-carbonized material. The specific pre-carbonization heating curve: the heating rate in the range of 0-600 (inclusive)°C (low temperature zone) is 30°C / min, the heating rate in the range of 600-900 (inclusive)°C (medium temperature zone) is 15°C / min, and the slow heating rate of 2°C / min is used for pre-carbonization in the range of 900-1100°C (high temperature zone). The pre-carbonized material was loaded into a graphite crucible, and graphitized for 24 hours at 2800°C in a medium frequency induction graphitization furnace to obtain anthracite-based artificial graphite primary particles. Next, the anthracite-based artificial graphite primary particles and oxidized asphalt (softening point 200°C) were mixed at room temperature in a mass ratio of 98:2, the mixer speed was 300rpm, and after mixing for 30min, the speed was reduced to 100rpm, and the granulation temperature was adjusted to 220°C for 60min, and finally it was carbonized for 1h at a heating rate of 5°C / min, a final temperature of 1300°C, and nitrogen protection, and finally anthracite-based artificial graphite secondary particles with a particle size of 20μm, that is, anthracite-based fast-charging graphite negative electrode materials, were obtained. It was assembled into a button-type half-cell with a specific capacity of 352.4mAh / g and a first coulombic efficiency of 93.1%; it was further assembled into a soft-pack battery with a lithium iron phosphate positive electrode, and its 5C / 0.2C rate performance was 86%.
[0040] Example 2
[0041] Anthracite (sulfur content of 1.2wt%) was crushed to a particle size of 80μm using a mechanical crushing method, and then the ash content was reduced to 2wt% by flotation. Then, the particle size was reduced to 5μm by a mechanical crusher, and then pre-carbonized by a gradient pre-carbonization program under an argon atmosphere, with a final pre-carbonization temperature of 1050°C to obtain a pre-carbonized material. The specific pre-carbonization heating curve: the heating rate in the range of 0-600 (inclusive)°C (low temperature zone) is 25°C / min, the heating rate in the range of 600-900 (inclusive)°C (medium temperature zone) is 18°C / min, and the slow heating rate of 3°C / min is used for pre-carbonization in the range of 900-1100°C (high temperature zone). The pre-carbonized material was loaded into a graphite crucible, and graphitized for 32 hours at 3200°C using an Acheson crucible graphitization furnace to obtain anthracite-based artificial graphite primary particles. Next, the anthracite-based artificial graphite primary particles were mixed with oxidized asphalt (softening point 240°C) at a mass ratio of 94:6 at room temperature, the mixer speed was 500rpm, and after mixing for 60min, the speed was reduced to 100rpm, and the granulation temperature was adjusted to 255°C for 60min, and finally, it was carbonized for 2h at a heating rate of 5°C / min, a final temperature of 1400°C, and nitrogen protection, and finally anthracite-based artificial graphite secondary particles with a particle size of 11μm, that is, anthracite-based fast-charging graphite negative electrode materials, were obtained. It was assembled into a button-type half-cell with a specific capacity of 365.2mAh / g and a first coulombic efficiency of 92.4%; it was further assembled into a soft-pack battery with a lithium iron phosphate positive electrode, and its 5C / 0.2C rate performance was 88.2%.
[0042] Example 3
[0043] Anthracite (sulfur content of 1.0wt%) was crushed to a particle size of D50200μm by mechanical crushing, and then the ash content was reduced to 5wt% by flotation. Then, the particle size was reduced to D50 of 8μm by a mechanical crusher, and then pre-carbonized by a gradient pre-carbonization program under an argon atmosphere, with a final pre-carbonization temperature of 1050°C to obtain a pre-carbonized material. The specific pre-carbonization heating curve: the heating rate in the range of 0-600 (inclusive)°C (low temperature zone) is 20°C / min, the heating rate in the range of 600-900 (inclusive)°C (medium temperature zone) is 10°C / min, and the slow heating rate of 5°C / min is used for pre-carbonization in the range of 900-1100°C (high temperature zone). The pre-carbonized material was loaded into a graphite crucible, and graphitized for 16 hours at 2900°C in a medium-frequency induction graphitization furnace to obtain anthracite-based artificial graphite primary particles. Next, the anthracite-based artificial graphite primary particles were mixed with oxidized asphalt (softening point 130°C) at a mass ratio of 90:10 at room temperature, the mixer speed was 150rpm, and after mixing for 45min, the speed was reduced to 80rpm, and the granulation temperature was adjusted to 150°C for 50min, and finally, it was carbonized for 2h at a heating rate of 5°C / min, a final temperature of 1200°C, and nitrogen protection, and finally anthracite-based artificial graphite secondary particles with a particle size of 17μm, that is, anthracite-based fast-charging graphite negative electrode materials, were obtained. It was assembled into a button-type half-cell with a specific capacity of 348.6mAh / g and a first coulombic efficiency of 92.2%; it was further assembled into a soft-pack battery with a lithium iron phosphate positive electrode, and its 5C / 0.2C rate performance was 89%.
[0044] Example 4
[0045] Anthracite (sulfur content of 3.0wt%) was crushed to a particle size of D50120μm by mechanical crushing, and then the ash content was reduced to 3wt% by flotation. Then, the particle size was reduced to D50 of 8μm by a mechanical crusher, and then pre-carbonized by a gradient pre-carbonization program in a helium atmosphere, with a final pre-carbonization temperature of 1050℃ to obtain a pre-carbonized material. The specific pre-carbonization heating curve: the heating rate in the range of 0-600 (inclusive)℃ (low temperature zone) is 26℃ / min, the heating rate in the range of 600-900 (inclusive)℃ (medium temperature zone) is 12℃ / min, and the range of 900-1100℃ (high temperature zone) is carbonized at a slow heating rate of 4℃ / min. The pre-carbonized material was loaded into a graphite crucible, and graphitized for 20h at 3100℃ in a box-type graphitization furnace to obtain anthracite-based artificial graphite primary particles. It was assembled into a button-type half-cell with a specific capacity of 360.8mAh / g and an initial coulombic efficiency of 92.8%. It was further matched with a lithium iron phosphate positive electrode and assembled into a soft-pack battery with a 5C / 0.2C rate performance of 85%.
[0046] Example 5
[0047] Anthracite (sulfur content of 2.5wt%) was crushed to a particle size of D50180μm by mechanical crushing, and then the ash content was reduced to 2.8wt% by flotation. Then, the particle size was reduced to D50 of 6μm by a mechanical crusher, and then pre-carbonized by a gradient pre-carbonization program under an argon atmosphere, with a final pre-carbonization temperature of 1050℃ to obtain a pre-carbonized material. The specific pre-carbonization heating curve: the heating rate in the range of 0-600 (inclusive)℃ (low temperature zone) is 28℃ / min, the heating rate in the range of 600-900 (inclusive)℃ (medium temperature zone) is 16℃ / min, and the range of 900-1100℃ (high temperature zone) is carbonized at a slow heating rate of 5℃ / min. The pre-carbonized material was loaded into a graphite crucible, and graphitized at 3000℃ for 20h in an internal string graphitization furnace to obtain anthracite-based artificial graphite primary particles. Next, the anthracite-based artificial graphite primary particles were mixed with bismaleimide (softening point 157°C) at a mass ratio of 98:2 at room temperature, the mixer speed was 300rpm, and after mixing for 30min, the speed was reduced to 50rpm, and the granulation temperature was adjusted to 170°C for 40min, and finally, it was carbonized for 2h at a heating rate of 5°C / min, a final temperature of 1400°C, and nitrogen protection, and finally anthracite-based artificial graphite secondary particles with a particle size of 13μm, that is, anthracite-based fast-charging graphite negative electrode materials, were obtained. It was assembled into a button-type half-cell with a specific capacity of 366.2mAh / g and a first coulombic efficiency of 94%; it was further assembled into a soft-pack battery with a lithium iron phosphate positive electrode, and its 5C / 0.2C rate performance was 88%.
[0048] Comparative Example 1
[0049] Low sulfur petroleum coke (<0.3wt%, ash content ≤0.5wt%) is crushed mechanically to a particle size D50 of 150μm, and then a mechanical crusher is used to reduce its particle size to D50 of 10μm, and then a gradient pre-carbonization program is used for pre-carbonization in a nitrogen atmosphere, and the final pre-carbonization temperature is 1050℃ to obtain a pre-carbonized material. The specific pre-carbonization heating curve: the heating rate in the range of 0-600 (inclusive)℃ (low temperature zone) is 25℃ / min, the heating rate in the range of 600-900 (inclusive)℃ (medium temperature zone) is 10℃ / min, and the range of 900-1100℃ (high temperature zone) is carbonized at a slow heating rate of 2℃ / min. The pre-carbonized material is loaded into a graphite crucible, and graphitized for 30h at 3000℃ in an Acheson graphitization furnace to obtain coke-based artificial graphite primary particles. Next, the coke-based artificial graphite primary particles were mixed with cross-linked asphalt (softening point 260°C) at a mass ratio of 95:5 at room temperature, the mixer speed was 280rpm, and after mixing for 30min, the speed was reduced to 60rpm, and the granulation temperature was adjusted to 280°C for 60min, and finally it was carbonized for 1h at a heating rate of 5°C / min, a final temperature of 1300°C, and nitrogen protection, and finally a coke-based fast-charging graphite negative electrode material with a particle size of 20μm was obtained. It was assembled into a button-type half-cell with a specific capacity of 358.2mAh / g and a first coulombic efficiency of 94.3%; it was further assembled into a soft-pack battery with a lithium iron phosphate positive electrode, and its 5C / 0.2C rate performance was 68%.
[0050] Comparative Example 2
[0051] Low-sulfur anthracite (sulfur content of 0.4wt%) was crushed to a particle size of 160μm by mechanical crushing, and then the ash content was reduced to 2wt% by flotation. Then, the particle size was reduced to 5μm by a mechanical crusher, and then, in an argon atmosphere, a gradient pre-carbonization program was used for pre-carbonization, and the final pre-carbonization temperature was 1050°C to obtain a pre-carbonized material. The specific pre-carbonization heating curve: the heating rate in the range of 0-600 (inclusive) ℃ (low temperature zone) is 25℃ / min, the heating rate in the range of 600-900 (inclusive) ℃ (medium temperature zone) is 10℃ / min, and the range of 900-1100℃ (high temperature zone) is carbonized at a slow heating rate of 3℃ / min. The pre-carbonized material was loaded into a graphite crucible, and graphitized at 3000℃ for 36h in an Acheson graphitization furnace to obtain anthracite-based artificial graphite primary particles. Next, the anthracite-based artificial graphite primary particles were mixed with cross-linked asphalt (softening point 260°C) at a mass ratio of 97:3 at room temperature, the mixer speed was 400rpm, and after mixing for 30min, the speed was reduced to 50rpm, and the granulation temperature was adjusted to 280°C for 60min, and finally it was carbonized for 2h at a heating rate of 5°C / min, a final temperature of 1400°C, and nitrogen protection, and finally anthracite-based artificial graphite secondary particles with a particle size of 11μm, that is, anthracite-based fast-charging graphite negative electrode materials, were obtained. It was assembled into a button-type half-cell with a specific capacity of 359.6mAh / g and a first coulombic efficiency of 93.6%; it was further assembled into a soft-pack battery with a lithium iron phosphate positive electrode, and its 5C / 0.2C rate performance was 75%.
[0052] Table 2
[0053]
[0054] The above description is only for better explaining the embodiments of the present invention, and is not intended to limit the present invention. Any modification or equivalent substitution that does not depart from the spirit and scope of the present invention shall fall within the scope of the present invention.
Claims
1. A method for preparing anthracite-based graphite negative electrode material, characterized in that: The following steps are involved: Step 1: subjecting the anthracite to mechanical crushing, flotation, and mechanical pulverization in sequence and then to gradient pre-carbonization treatment to obtain pre-carbonized material; Step 2: Graphitizing the pre-carbonized material to obtain anthracite-based artificial graphite primary particles.
2. The method for preparing an anthracite-based graphite negative electrode material according to claim 1, characterized in that: The method also includes step 3: mixing the anthracite-based artificial graphite primary particles with a binder, and then mechanically granulating them under heating conditions, and obtaining anthracite-based artificial graphite secondary particles by carbonization.
3. The method for preparing an anthracite-based graphite negative electrode material according to claim 1, characterized in that: The sulfur content of the anthracite is 1-3wt%; the particle size D50 of the anthracite after mechanical crushing is 75-200μm, the ash content after flotation is 2-5wt%, and the particle size D50 after mechanical crushing is 5-10μm.
4. The method for preparing an anthracite-based graphite negative electrode material according to claim 1, characterized in that: The specific conditions of the gradient pre-carbonization treatment are: carried out under argon or helium, the final pre-carbonization temperature is 1050°C, and the gradient pre-carbonization curve is: the heating rate in the range of 0-600°C is 20-30°C / min, the heating rate in the range of 600-900°C is 10-18°C, and the heating rate in the range of 900-1100°C is 2-5°C / min.
5. The method for preparing an anthracite-based graphite negative electrode material according to claim 1, characterized in that: The specific conditions of the graphitization treatment are as follows: the graphitization temperature is 2800-3200° C., the graphitization time is 16-32 hours, and the graphitization furnace is one of an induction vacuum graphitization furnace, an Acheson crucible furnace, an Acheson box furnace or an Acheson inner series furnace.
6. The method for preparing an anthracite-based graphite negative electrode material according to claim 2, characterized in that: The binder is one of oxidized asphalt, cross-linked asphalt, phenolic resin, epoxy resin, polyester resin, vinyl ester, bismaleamide, polyimide, and cyanate ester.
7. The method for preparing an anthracite-based graphite negative electrode material according to claim 2, characterized in that: The specific process of the mechanical granulation is: anthracite-based artificial graphite primary particles and a binder are mixed at a mass ratio of (90-98): (2-10) at a high speed of 150-500 rpm at room temperature for 30-60 minutes, then the rotation speed is reduced to 20-100 rpm, and heated to 150-300°C for fusion granulation for 30-60 minutes; the specific conditions of the carbonization are: in a nitrogen atmosphere, the carbonization treatment is carried out at a heating rate of 5°C / min for 1-2 hours, and the final carbonization temperature is 1200-1400°C.
8. An anthracite-based graphite negative electrode material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The invention comprises anthracite-based artificial graphite primary particles with a particle size D50 of 5-10 μm and anthracite-based artificial graphite secondary particles with a particle size D50 of 11-20 μm.
9. A negative electrode material for a lithium ion battery, characterized in that: Including the anthracite-based graphite negative electrode material as described in claim 8.
10. A lithium ion battery, characterized in that: The negative electrode material for a lithium-ion battery comprises the negative electrode material of claim 9.
Citation Information
Patent Citations
Coal-based active coke hole structure grouping regulation method based on coal internal ash catalytic activation
CN110171826A
Artificial composite graphite negative electrode material, lithium ion battery, preparation method and application
CN111244453A
Preparation method of artificial graphite negative electrode material
CN113912054A
Preparation method of graphite negative electrode material as well as product and application of graphite negative electrode material
CN114477162A
Coal raw material lithium ion battery negative electrode material and preparation method thereof
CN115744892A
Cited By
Preparation of multi-coal-type synergistic fast-charging graphite negative electrode material and lithium ion battery
CN121672511A
Preparation of multi-coal synergistic fast-charging graphite negative electrode material and lithium ion battery
CN121672511B