Method and device for preparing composite phase gypsum with adjustable and controllable phase components from ardealite
Through the technical means of vibration screening, Venturi drying, calcined fluidized bed, impingement flow cooling and aging fluidized bed, the phase component ratio of phosphogypsum is accurately adjusted, which solves the problem of poor control accuracy in the preparation of composite phase gypsum by calcination of phosphogypsum. And the problem of low cooling efficiency improves the utilization rate of phosphogypsum resources.
Patent Information
- Application Number
- CN202410910749.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-29
AI Technical Summary
In the process of preparing composite-phase gypsum by calcining phosphogypsum, the existing technology has problems such as poor accuracy in regulating the proportion of each phase component, single adjustment means, low cooling and aging efficiency, and poor product stability, resulting in low resource utilization of phosphogypsum.
The technical means of vibration screening, Venturi drying, calcined fluidized bed, impingement flow cooling and aging fluidized bed are used to achieve the preparation of high-temperature composite phase gypsum powder of phosphogypsum by controlling the fluidization state and gas flow rate. The ball mill modifies the particle size, combined with gas mixing control, to accurately adjust the component ratios of the AII phase, HH phase, AIII phase and DH phase.
It achieves precise control of the content of each phase component of composite phase gypsum, improves the calcination cooling rate and aging efficiency, reduces energy consumption, ensures the stability and quality of the product, and solves the problem of low resource utilization of phosphogypsum.
Smart Images

Figure CN118851602A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of phosphogypsum resource utilization, and in particular to a method and a device for preparing composite phase gypsum with adjustable phase components from phosphogypsum. Background Art
[0002] Phosphogypsum is a typical industrial by-product gypsum. More than 95% of my country's phosphogypsum comes from the production of dihydrate wet phosphoric acid. Every ton of phosphoric acid produced produces 4.5 to 5.5 tons of phosphogypsum. At present, the cumulative stockpile of phosphogypsum in my country has reached 800 million tons, and the comprehensive utilization rate is less than 50%. The large-scale storage of phosphogypsum has brought about environmental pollution problems such as water, land and air, and has become a bottleneck restricting the development of phosphorus chemical enterprises.
[0003] Phosphogypsum is similar to natural gypsum. Its main component, calcium sulfate dihydrate, contains 85-90% of it. It can replace natural gypsum to prepare phosphogypsum-based building material powder. However, the impurities in phosphogypsum are complex and diverse, especially water-soluble impurities such as phosphorus and fluorine, which will have a negative impact on the gelling properties of phosphogypsum-based building gypsum. In order to improve the resource utilization of phosphogypsum in the preparation of building gypsum powder materials by calcining phosphogypsum, phosphogypsum must be purified at the front end. At present, most domestic phosphogypsum calcining companies use water washing purification. The water washing purification process will cause secondary pollution, and some phosphating companies have water balance problems, and water washing purification cannot be achieved.
[0004] In order to break through the limitations of wet purification, high-temperature calcination is often used to improve the performance of phosphogypsum. After medium and high temperature calcination, phosphogypsum can not only effectively remove or reduce harmful impurities, but also prepare type II anhydrous gypsum with high strength, water resistance and rheology that are much better than building gypsum. The cementing performance advantage of type II anhydrous gypsum makes up for the defect that impurities in phosphogypsum have a negative impact on performance. Type II anhydrous gypsum is divided into S type (350-650℃), U type (650-750℃) and E type (750-1180℃) according to the different calcination preparation temperatures. There are significant differences in the hydration activity of different types of type II anhydrous gypsum. However, the key technical bottleneck of fully utilizing type II anhydrous gypsum as a cementing material to stimulate hydration activity has not been solved in China, and there are problems such as low early strength, low hydration activity stimulation efficiency and easy to cause frosting in the later stage.
[0005] In order to overcome the above problems, the idea of preparing composite phase gypsum of type II anhydrous gypsum and β-hemihydrate gypsum by calcining phosphogypsum is proposed. When composite phase gypsum is used as the base powder of downstream mortar products, it can give full play to the performance advantages of type II anhydrous gypsum and β-hemihydrate gypsum under the deployment of reasonable admixtures. β-hemihydrate gypsum provides early strength, and type II anhydrous gypsum provides later strength and water resistance. The proportions of type II anhydrous gypsum phase (AII phase) and β-hemihydrate gypsum phase (HH phase) in composite phase gypsum are different, and the cementing properties of composite phase gypsum are also different. Since the phase transition during the calcination of phosphogypsum is continuous and gradual, a large amount of type III anhydrous gypsum will inevitably be produced when type II anhydrous gypsum is produced. At the same time, for some processes with poor calcination sufficiency, some dihydrate gypsum will also exist in the composite phase gypsum. The content of type III anhydrous gypsum phase (AIII phase) and dihydrate gypsum phase (DH phase) and the content of AII phase components have a great influence on the cementitious properties of composite phase gypsum, and directly affect the rheological properties, strength properties, and product stability of composite phase gypsum-based mortar slurry. Therefore, the proportion and stability control of each phase component in the composite phase gypsum is the key to satisfying the composite phase gypsum as a gypsum-based powder cementitious material.
[0006] At present, the domestic process technology for calcining phosphogypsum to prepare composite phase gypsum has the following problems: it is impossible to achieve precise control of the proportion of each phase component in the composite phase gypsum; the means for adjusting the proportion of the AII phase component in the composite phase gypsum is single; the conversion efficiency of the AIII phase to the HH phase in the composite phase gypsum is low, and the DH phase content will increase during the aging process; the existing aging technology has the problems of long aging cycle and low aging efficiency; the calcined gypsum has a slow cooling speed and a long cooling process; the heat gradient utilization is poor, the calcination process has high energy consumption and poor continuity. Summary of the invention
[0007] The object of the present invention is to provide a method and device for preparing composite phase gypsum with adjustable phase components from phosphogypsum, so as to solve the problems of poor precision in controlling the proportion of each phase component, single adjustment means, low cooling and aging efficiency and poor product stability existing in the process of preparing composite phase gypsum in the prior art.
[0008] In order to solve the above technical problems, the present invention adopts the following technical solution: a method for preparing composite phase gypsum with adjustable phase components from phosphogypsum, characterized by comprising the following steps:
[0009] S1. The phosphogypsum raw material with a free water content of less than 6% is screened by a vibrating screening device, and the screened phosphogypsum enters a venturi dryer through a metering screw feeder, and enters a cyclone separator after drying. The separated phosphogypsum powder enters a calcining fluidized bed;
[0010] S2. The phosphogypsum powder enters from the feed port of the left chamber of the calcining fluidized bed, and the hot air enters from the bottom of the calcining fluidized bed. After the phosphogypsum powder contacts the hot air with a flow rate of 0.5 to 5 m / s, it enters the right chamber from the connection point at the bottom of the left chamber in a fluidized state, and is finally discharged from the upper discharge port of the right chamber. The calcination temperature of the fluidized phosphogypsum powder is controlled to be 300 to 450° C., and the residence time in the calcining fluidized bed is 30 to 90 min, to prepare a high-temperature composite phase gypsum powder;
[0011] S3. The high-temperature composite phase gypsum powder enters the impinging flow cooler at a flow rate of 8 to 12 m / s, and after being collided with the cooling air at a flow rate of 14 to 20 m / s and cooled, enters the cyclone cooler to further cool the composite phase gypsum powder to below 70°C. The hot air after heat exchange in the cyclone cooler is dedusted by the second bag filter;
[0012] S4. The composite phase gypsum powder after cooling enters the ball mill for ball milling modification of the appearance and particle size of the composite phase gypsum powder particles, and the particle size distribution range after modification is controlled to be between 38 and 75 μm. The modified composite phase gypsum powder is sent to the buffer bin for temporary storage;
[0013] S5. After the compressed air is humidified, it is mixed with the hot air after dust removal by the second bag dust collector in a gas mixing tank to obtain a mixed gas with a temperature of 25-60°C and a relative humidity of 40-90%. The mixed gas is sent into the aging fluidized bed from the bottom, and the composite phase gypsum powder in the buffer bin enters from the feed port of the left chamber of the aging fluidized bed. After contacting with the mixed gas with a flow rate of 0.5-3m / s, it becomes fluidized. Since the bottom of the left chamber is connected with the bottom of the right chamber, the composite phase gypsum powder enters the right chamber from the connection, and is finally discharged from the upper discharge port of the right chamber to the finished product bin. The composite phase gypsum powder in the fluidized state is controlled to stay in the aging fluidized bed for 50-150min to obtain a composite phase gypsum finished product. The exhaust gas of the aging fluidized bed enters the first bag dust collector.
[0014] A further technical solution is that the content of calcium sulfate dihydrate in the phosphogypsum raw material in step S1 is ≥85%, the pH value is ≥3.0, and before screening, it is intermittently turned over and homogenized and dried with a grab bucket; the aperture of the vibrating screening equipment is ≤3cm.
[0015] A further technical solution is that hot air with a temperature of 150-200°C and a gas velocity of 15-20m / s is introduced from the bottom of the Venturi dryer in step S1, and the hot air is provided by a coal-fired hot air furnace; the tail gas of the cyclone separator is sent to the first bag dust collector.
[0016] A further technical solution is that the hot air in step S2 is provided by a natural gas hot air furnace.
[0017] A further technical solution is that the cooling air in step S3 is provided by a fan as natural wind.
[0018] A further technical solution is that pneumatic valves are provided at the discharge ports of the calcining fluidized bed and the aging fluidized bed, and the opening of the pneumatic valves is 50-100%.
[0019] A further technical solution is that the AII phase content in the composite phase gypsum product is 10-90%, the HH phase content is 5-85%, the DH phase is 0.5-1.5%, the AIII phase content is 0-0.5%, and the attached water content is 0-1.0%.
[0020] A further technical solution is that the device used in the method includes a vibrating screening device, a metering screw feeder, a Venturi dryer, a cyclone separator, a calcining fluidized bed, an impinging flow cooler, a cyclone cooler, a ball mill, a buffer bin, an aging fluidized bed, and a finished product bin connected in sequence; the air inlet of the Venturi dryer is connected to the air outlet of the coal-fired hot blast furnace, and the air outlet of the cyclone separator is connected to the air inlet of the first bag dust collector; the top exhaust port of the calcining fluidized bed is connected to the air inlet of the natural gas hot blast furnace through an exhaust gas pipeline, and the bottom air inlet is connected to the air outlet of the natural gas hot blast furnace; the air inlet of the impinging flow cooler is connected to the fan, the discharge port of the impinging flow cooler is connected to the feed port of the cyclone cooler, and the air outlet of the cyclone cooler is connected to the air inlet of the gas mixing tank through the second bag dust collector; the top exhaust port of the aging fluidized bed is connected to the first bag dust collector through the exhaust gas pipeline, and the bottom air inlet is connected to the air outlet of the gas mixing tank; the air inlet of the gas mixing tank is connected to the gas humidifying tank and the air compressor in sequence.
[0021] A further technical solution is that the impinging flow cooler comprises an upper separation chamber and a lower impingement chamber, the separation chamber and the impingement chamber are connected, a feed nozzle and an air intake nozzle are arranged opposite to each other on both sides of the impingement chamber, a discharge port is arranged at the bottom of the impingement chamber, an exhaust port is arranged at the top of the separation chamber, and the exhaust port is connected to the air inlet of the coal-fired hot air furnace after passing through a dust separation device.
[0022] A further technical solution is that the diameter of the pipe at the connection between the separation chamber and the impact chamber is 1 / 10 to 1 / 20 of the inner diameter of the impact chamber.
[0023] Working mechanism:
[0024] (1) Raw material pretreatment stage: The phosphogypsum raw materials are homogenized by stacking and turning the pile with a grab bucket, so that the free water content of the phosphogypsum is reduced to a certain range while ensuring the uniformity of the material properties. The treated phosphogypsum is passed through a vibrating screening device with a certain sieve aperture, and the phosphogypsum on the sieve is returned to the raw material warehouse, and the screened material enters the Venturi drying system through a metering screw feeder, effectively avoiding the problem of material blockage during the process of the phosphogypsum material entering the Venturi drying system through the metering screw, and ensuring the continuity and stability of the system feed. The phosphogypsum after homogenization pretreatment ensures the stability of the total heat required by the system during the fluidized calcination process to a certain extent, avoiding large temperature fluctuations, which would cause large deviations in the phase components of the composite phase gypsum.
[0025] (2) Fluidized graded calcination stage: The lower end of the Venturi dryer is introduced with hot flue gas of a certain temperature provided by a coal-fired hot blast furnace. After being accelerated by the Venturi, the agglomerated phosphogypsum conveyed by the metering screw is quickly dispersed and the free water of the phosphogypsum is removed. Finally, it is blown out from the upper end of the Venturi dryer in the form of a gas-solid fluid. After the high-humidity gas and the phosphogypsum powder are separated by a cyclone separator, it enters the calcination fluidized bed, where it is mixed with the hot air provided by the natural gas hot blast furnace and fluidized, thereby achieving rapid heating of the phosphogypsum powder in the calcination fluidized bed, reducing the energy loss of heating the wet gas, and at the same time ensuring the uniformity of the crystal water removal rate of the phosphogypsum powder, thereby ensuring the stability of the phase change rate, and realizing the gradual transformation of the DH phase in the phosphogypsum into the HH phase, AIII phase and AII phase. By using natural gas to heat air as fluidizing air, the temperature of the hot air entering the calcination fluidized bed is accurately controlled. By regulating the temperature and wind speed of the fluidizing air at the bottom of the calcination fluidized bed, the actual calcination temperature of the phosphogypsum powder material in the fluidized bed is controlled, and ultimately the precise control of the AII phase and DH phase content of phosphogypsum during the calcination process is achieved.
[0026] (3) Impingement flow cooling and modification stage: The high-temperature composite phase gypsum powder prepared by fluidized bed calcination and the cooling air enter the impingement flow cooler from the nozzle at a certain flow rate respectively. The two jets collide with each other in the impact chamber 807 at an extremely high flow rate to form a large contact area, thereby accelerating the cooling rate of the high-temperature composite phase gypsum powder. The composite phase gypsum powder then enters the cyclone cooler for further cooling, and finally enters the ball mill for modification of the appearance morphology and particle size of the composite phase gypsum powder particles. The modified composite phase gypsum powder enters the buffer bin.
[0027] The gas-solid hot fluid formed by the high-temperature composite phase gypsum and the cold air form an impact flow effect. The hot gypsum flow and the cold air flow collide with each other at high speed, forming a high turbulence in the impact chamber 807 and reaching a very high relative velocity between the phases, increasing the effective contact area of the fluid, thereby strengthening the transfer of heat between the phases, increasing the transfer rate of gypsum heat to the gas phase, and realizing rapid heat dissipation and cooling of high-temperature gypsum. The gypsum particles are converted into radial flow due to the collision and are discharged by gravity.
[0028] (4) Rapid aging stage: The compressed air humidified by the gas humidification tank and the heat exchange gas after dust removal from the cyclone cooler enter the gas mixing tank for uniform mixing. The mixed gas is used as fluidizing air to quickly age the modified composite phase gypsum powder entering the aging fluidized bed from the buffer bin. Since the modified composite phase gypsum powder is always in a fluidized state in the aging fluidized bed, the contact efficiency and uniformity between the modified composite phase gypsum powder and the mixed gas are enhanced, and the efficiency of the AIII phase in the modified composite phase gypsum powder absorbing the gaseous water in the mixed gas to the HH phase is accelerated, while effectively avoiding the problem of poor material uniformity caused by the aging dead zone. After aging, the modified composite phase gypsum powder enters the finished product bin, and the exhaust gas generated enters the bag dust removal equipment.
[0029] During the aging process of calcined gypsum, each phase component will transform into each other: AIII phase has high hydration activity and poor stability, and it is very easy to absorb gaseous water in the air and transform into HH phase; HH phase will also transform into DH phase under certain conditions; AII has good stability compared to AIII and HH phases, and will not undergo phase transformation even in an environment with high humidity air; The efficiency of transformation from AIII phase to HH phase is mainly affected by the temperature, relative humidity and aging time of the aging gas. In the present invention, the fluidizing air used in the aging fluidized bed is a binary mixed gas composed of humidified compressed air and low-temperature cyclone cooling air. The temperature and relative humidity in the binary mixed gas are regulated, and the aging residence time of the composite phase gypsum in the aging fluidized bed is regulated by controlling the fluidizing air flow rate at the bottom of the aging fluidized bed and the valve opening of the discharge port. Finally, the control of the kinetic process of the transformation from AIII phase to HH phase is achieved, thereby realizing the precise regulation of the AIII phase, HH phase and DH phase components of the composite phase gypsum during the aging process.
[0030] Both the calcination fluidized bed and the aging fluidized bed are two-chamber fluidized beds, with gypsum powder flowing in from the left chamber and out from the right chamber. After the material enters the bed, it forms a fluidized state under the action of the fluidizing wind at the bottom. Due to the principle of the left and right chambers of the fluidized bed forming a communicating vessel, the fluidization heights of the materials in the left and right chambers tend to be consistent under the fluidization state. Under the condition of constant flow rate, as the phosphogypsum powder continuously enters the fluidized bed, the fluidization height of the phosphogypsum powder increases, and when the fluidization height reaches the height of the discharge port, the material is continuously discharged.
[0031] The hot air coming out of the separation chamber at the top of the calcining fluidized bed is used as the air source for the natural gas hot blast furnace, the heat exchange air after being cooled by the impingement flow is used as the air source for the coal-fired hot blast furnace, and part of the hot air after being cooled by the cyclone is used as the fluidizing air source for the aging fluidized bed. The heat of the entire system is utilized in a cascade manner, reducing the heat loss of the system and thus reducing the energy consumption of the system.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] (1) The phosphogypsum is initially dehydrated and dried by a venturi dryer. After separation by a cyclone separator, the phosphogypsum powder enters a calcining fluidized bed, where it is mixed with hot air provided by a natural gas hot blast furnace and fluidized, thereby achieving rapid heating of the phosphogypsum powder in the calcining fluidized bed, and gradually transforming the DH phase in the phosphogypsum into the HH phase, the AIII phase, and the AII phase. The high-temperature composite phase gypsum powder is mixed with the cooling air at high speed in an impact flow cooler, rapidly cooled and further cooled, and then modified by ball milling. It is uniformly contacted with the mixed gas in the aging fluidized bed, which accelerates the efficiency of the AIII phase in the modified composite phase gypsum powder absorbing the gaseous water in the mixed gas and transforming into the HH phase. At the same time, the problem of poor material uniformity caused by the aging dead zone is effectively avoided, thereby obtaining high-quality composite phase gypsum with high total content of the AII phase and the HH phase and low total content of the DH phase and the AIII phase.
[0034] (2) The device is composed of a vibration screening device, a metering screw feeder, a venturi dryer, a cyclone separator, a calcination fluidized bed, an impinging flow cooler, a cyclone cooler, a ball mill, a buffer bin, an aging fluidized bed, and a finished product bin, which are connected in sequence to achieve continuous production of composite phase gypsum and precise control of the content of each phase component. The fluidized bed is used to ensure good material uniformity and small dead zone during the calcination and aging processes, thereby ensuring the stability of product quality.
[0035] (3) Compared with the traditional method of preparing complex phase gypsum powder, the phosphogypsum powder is in a gas-solid fluid state during the calcination, cooling and aging processes, which enhances the mass transfer, heat transfer and phase conversion efficiency of the entire process. By regulating the temperature and residence time during the fluidized calcination of phosphogypsum, controlling the rapid cooling rate under the impact flow effect, and controlling the gas temperature, humidity and residence time during the rapid aging process, precise control of the phase components of the complex phase gypsum can be achieved. The method and device can continuously realize the precise control of the content of each gypsum phase component in the complex phase gypsum, with a wide control range. The prepared complex phase gypsum has good phase uniformity, fast cooling rate of calcined gypsum, high heat dissipation efficiency, short process flow, short aging cycle, high aging efficiency, cascade utilization of system heat, high thermal efficiency and low comprehensive energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a structural schematic diagram of the present invention.
[0037] Figure 2 It is a schematic diagram of the structure of the impact cooling reactor in the present invention.
[0038] In the figure: 1-vibration screening equipment, 2-metering screw feeder, 3-coal-fired hot air furnace, 4-Venturi dryer, 5-cyclone separator, 6-calcination fluidized bed, 7-natural gas hot air furnace, 8-impinging flow cooler, 801-exhaust port, 802-thermometer, 803-pressure gauge, 804-separation chamber, 805-feed nozzle, 806-intake nozzle, 807-impingement chamber, 808-discharge port, 9-cyclone cooler, 10-ball mill, 11-fan, 12-first bag dust collector, 13-second bag dust collector, 14-buffer bin, 15-aging fluidized bed, 16-gas control cabinet, 17-gas mixing tank, 18-gas humidifying tank, 19-air compressor, 20-finished product bin, 21-pneumatic valve, 22-dust separation device. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0040] Example 1
[0041] Figure 1 The invention shows a device for preparing composite phase gypsum with adjustable phase components from phosphogypsum, which includes a vibration screening device 1, a metering screw feeder 2, a venturi dryer 4, a cyclone separator 5, a calcining fluidized bed 6, an impinging flow cooler 8, a cyclone cooler 9, a ball mill 10, a buffer bin 14, an aging fluidized bed 15, and a finished product bin 20, which are connected in sequence. The air inlet of the venturi dryer 4 is connected to the air outlet of the coal-fired hot air furnace 3, and the air outlet of the cyclone separator 5 is connected to the air inlet of the first bag filter 12. The top exhaust port of the calcining fluidized bed 6 is connected to the air inlet of the natural gas hot air furnace 7 through the tail gas pipeline, and the bottom air inlet is connected to the air outlet of the natural gas hot air furnace 7. The left chamber of the calcining fluidized bed 6 is provided with a feed port, and the right chamber is provided with a discharge port. The bottoms of the left and right chambers are connected. A pneumatic valve 21 is installed on the pipe connected to the discharge port. The feed port is connected to the discharge port of the cyclone separator 5, and the discharge port is connected to the feed port of the impinging flow cooler 8. The air inlet of the impinging flow cooler 8 is connected to the fan 11, and the discharge port is connected to the feed port of the cyclone cooler 9. The gas separated by the second bag dust collector 13 at the air outlet of the cyclone cooler 9 is connected to the air inlet of the gas mixing tank 17 through the gas control cabinet 16, and the discharge port of the cyclone cooler 9 is connected to the ball mill 10. The air inlet of the gas mixing tank 17 is connected to the gas humidification tank 18 and the air compressor 19 in sequence.
[0042] like Figure 2As shown, the impinging flow cooler 8 comprises an upper separation chamber 804 and a lower impinging chamber 807, the separation chamber 804 and the impinging chamber 807 are connected, and a feed nozzle 805 and an air inlet nozzle 806 are arranged on both sides of the impinging chamber 807, a discharge port 808 is arranged at the bottom of the impinging chamber 807, and an exhaust port 801 is arranged at the top of the separation chamber 804, and the exhaust port 801 is connected to the air inlet of the coal-fired hot air furnace 3 through the dust separation device 22. In order to facilitate gas-solid separation, the pipe diameter at the connection between the separation chamber 804 and the impinging chamber 807 is 1 / 10 to 1 / 20 of the inner diameter of the impinging chamber 807. The dust separation device 22 can be a bag dust collector, or a separation device with a partition baffle arranged in a hollow cavity. After the gas with a small amount of dust enters the dust separation device 22, it impacts on the partition baffle and settles under the action of gravity, thereby realizing dust separation, so that cleaner gas enters the coal-fired hot air furnace 3.
[0043] After homogenization, the phosphogypsum raw material passes through the vibrating screening device 1, and then enters the hopper of the metering screw feeder 2 through the conveyor belt. The metered phosphogypsum is transported to the venturi dryer 4, and dispersed and free water is removed in the hot flue gas generated by the coal-fired hot blast furnace 3, and then enters the cyclone separator 5 in the form of gas-solid fluid to separate the high-humidity gas from the phosphogypsum powder. The high-humidity gas is discharged after passing through the first bag filter 12. The phosphogypsum powder enters the calcining fluidized bed 6, and while forming a fluidized state in the hot air generated by the natural gas hot blast furnace 7, the DH phase gradually transforms into the HH phase, the AIII phase and the AII phase to form a composite phase gypsum. The hot air generated during the calcination process flows back to the natural gas hot blast furnace 7 as part of the gas source.
[0044] After the high-temperature composite phase gypsum powder comes out of the calcining fluidized bed 6, it enters the impinging flow cooler 8 through the feed nozzle 805. The cooling air generated by the fan 11 enters from the air inlet nozzle 806 and forms an impinging flow for rapid heat exchange cooling in the impinging chamber 807. During the impinging flow cooling and heat exchange process, the thermometer 802 and the pressure gauge 803 at the top of the separation chamber 804 respectively monitor the temperature and pressure in real time.
[0045] The hot air generated by cooling passes through the separation chamber 804 for gas-solid separation and then flows back from the top exhaust port 801 as part of the air source of the coal-fired hot blast furnace 3. The cooled composite phase gypsum powder is discharged from the discharge port 808 and enters the cyclone cooler 9 for further cooling and separation. The hot gas separated by the cyclone cooler 9 is dedusted by the second bag filter 13, and then enters the gas mixing tank 17 after passing through the gas control cabinet 16. The cooled composite phase gypsum powder enters the ball mill 10 for ball milling modification, and the modified composite phase gypsum powder enters the buffer bin 14. The compressed air generated by the air compressor 19 passes through another gas control cabinet and enters the gas humidification tank 18 for humidification, and then enters the gas mixing tank 17 and mixes with the hot gas generated by the cyclone cooler 9 to serve as the fluidizing air of the aging fluidized bed 15. The modified composite gypsum powder from the buffer bin 14 enters the aging fluidized bed 15 and forms a fluidized state under the action of the fluidizing wind at the bottom. The AIII phase in the modified composite gypsum powder absorbs the gaseous water in the fluidizing wind and is converted into the HH phase to achieve rapid aging. The aged modified composite gypsum powder enters the finished product bin 20 for sealed storage.
[0046] Example 2
[0047] The composite phase gypsum was prepared using the device in Example 1. The treatment object of this example was phosphogypsum produced during the wet production of phosphoric acid in a phosphoric acid plant. The analysis results are as follows.
[0048] Test items Adherent water Crystal water grade pH result / % 18 18.8 87 3.2
[0049] The target phase components of the composite phase gypsum powder prepared from phosphogypsum are shown in the following table.
[0050] Test items Phase AIII / adherent water AII phase DH phase HH phase result / % <1% 30±3% <1.5% 55±3%
[0051] (1) Raw material pretreatment stage: During the storage period, the phosphogypsum raw materials are intermittently turned by a grab bucket to reduce the free water content of the phosphogypsum to 6%. The phosphogypsum after homogenization is passed through a vibrating screening device 1 with a circular screen with a diameter of 3 cm. The phosphogypsum under the screen enters the lower end of the Venturi dryer 4 through a metering screw feeder 2.
[0052] (2) Fluidized graded calcination stage: The hot flue gas at 180°C provided by the coal-fired hot blast furnace 3 enters from the lower end of the venturi dryer 4 at a flow rate of 18 m / s. After being accelerated, the hot air breaks up the agglomerated phosphogypsum and removes the free water of the phosphogypsum. It is blown out from the upper end in the form of gas-solid fluid and enters the cyclone separator 5. The high-humidity gas enters the first bag filter 12 from the top outlet of the cyclone separator 5. The phosphogypsum powder coming out of the bottom enters from the feed port on the left chamber of the calcination fluidized bed 6. The hot air generated by the natural gas hot blast furnace 7 enters from the two air inlets at the bottom of the calcination fluidized bed 6 and passes through the air distribution plate at a flow rate of 2.2 m / s to fluidize the phosphogypsum powder. The phosphogypsum powder in the left chamber enters the right chamber from the bottom connection, and the material level height tends to be consistent under the action of the fluidizing air. As the phosphogypsum powder continuously enters the left chamber, the material level in the right chamber also rises. When the material level reaches the height of the upper discharge port of the right chamber, the calcined composite phase gypsum powder is continuously discharged. During the fluidized calcination process of the phosphogypsum powder, the material temperature is controlled at 375±5℃, the pneumatic valve opening is 100%, and the residence time is 40±3min. The DH phase in the phosphogypsum powder gradually transforms into the HH phase, AIII phase and AII phase. The AII phase content in the prepared composite phase gypsum powder is 30±3%, and the DH phase content is less than 1.0%.
[0053] (3) Impingement flow cooling and modification stage: The high-temperature composite phase gypsum powder from the calcining fluidized bed 6 passes through the 38 mm feed nozzle 805 and enters the impingement chamber 807 of the impingement flow cooler 8 at a flow rate of 11 m / s. At the same time, the cooling air passes through the 24 mm air inlet nozzle 806 and enters the impingement chamber 807 at a flow rate of 18 m / s. The impact forms a large contact area and high turbulence and reaches a high relative velocity between phases, which strengthens the heat transfer of the high-temperature composite phase gypsum powder and accelerates the cooling rate of the high-temperature composite phase gypsum powder. The temperature of the composite phase gypsum powder is reduced to 105°C in a short time, and then enters the cyclone cooler 9. After cyclone cooling, the temperature of the composite phase gypsum powder is further reduced to 57°C. Finally, it enters the ball mill 10 for ball milling modification to a particle size distribution range of 38 to 75 μm. The modified composite phase gypsum powder enters the buffer bin 14.
[0054] (4) Rapid aging stage: The compressed air generated by the air compressor 19 enters the gas humidification tank 18 through the gas control cabinet, and the humidified gas with a relative humidity of 95% enters the gas mixing tank 17. At the same time, the hot gas with a temperature of 50°C and a relative humidity of 25% coming out of the cyclone cooler 9 also enters the gas mixing tank 17 from another air inlet of the gas mixing tank. The volume flow ratio of the humidified gas to the hot gas is 4:1, and the temperature of the formed mixed gas is 35°C and the relative humidity is 81%. The mixed gas enters from the bottom of the aging fluidized bed 15 after passing through the gas control cabinet, and is used as fluidizing air after passing through the air distribution plate, with a gas velocity of 1.5m / s. The composite phase gypsum powder in the buffer bin 14 continuously enters the fluidized bed from the left chamber feed port of the aging fluidized bed 15. Under the action of the fluidizing wind, the composite phase gypsum powder is in a fluidized state. The AIII phase in the composite phase gypsum powder absorbs the gaseous water in the binary mixed gas and transforms into the HH phase. After 70 minutes of aging, the fluidization height of the composite phase gypsum powder reaches the designed height of the right chamber discharge port, and the composite phase gypsum powder is continuously discharged into the finished product bin 20. The tail gas generated by the aging fluidized bed 15 enters the first bag dust removal stage 12.
[0055] The test results of the phase components of the composite phase gypsum powder prepared by the above process are shown in the following table, which meets the requirements of the target phase component control.
[0056]
[0057]
[0058] Example 3
[0059] The composite phase gypsum was prepared by using the device in Example 1. The treatment object in this example was desulfurized gypsum produced by flue gas desulfurization in a chemical plant. The analysis results are as follows.
[0060] Test items Adherent water Crystal water grade pH result / % 16 20.1 95 6.7
[0061] The target phase components of the composite phase gypsum powder prepared from phosphogypsum are shown in the following table.
[0062] Test items Phase AIII / adherent water AII phase DH phase HH phase result / % <1% 15±3% <1.5% 80±3%
[0063] (1) Raw material pretreatment stage: During the storage period, the phosphogypsum raw materials are intermittently turned by a grab bucket to reduce the free water content of the phosphogypsum to 5.5%. The homogenized phosphogypsum passes through a vibrating screening device 1 with a circular screen with a diameter of 2.5 cm. The phosphogypsum under the screen enters the lower end of the Venturi dryer 4 through a metering screw feeder 2.
[0064] (2) Fluidized graded calcination stage: The hot flue gas at 150°C provided by the coal-fired hot blast furnace 3 enters from the lower end of the venturi dryer 4 at a flow rate of 15 m / s. After being accelerated, the hot air breaks up the agglomerated phosphogypsum and removes the free water of the phosphogypsum. It is blown out from the upper end in the form of gas-solid fluid and enters the cyclone separator 5. The high-humidity gas enters the first bag filter 12 from the top outlet of the cyclone separator 5. The phosphogypsum powder coming out of the bottom enters from the feed port on the left chamber of the calcination fluidized bed 6. The hot air generated by the natural gas hot blast furnace 7 enters from the two air inlets at the bottom of the calcination fluidized bed 6 and passes through the air distribution plate at a flow rate of 2.5 m / s to fluidize the phosphogypsum powder. The phosphogypsum powder in the left chamber enters the right chamber from the bottom connection, and the material level height tends to be consistent under the action of the fluidizing air. As the phosphogypsum powder continuously enters the left chamber, the material level in the right chamber also rises. When the material level reaches the height of the upper discharge port of the right chamber, the calcined composite phase gypsum powder is continuously discharged. During the fluidized calcination process of the phosphogypsum powder, the material temperature is controlled at 340±5℃, the pneumatic valve opening is 95%, and the residence time is 40±3min. The DH phase in the phosphogypsum powder gradually transforms into the HH phase, AIII phase and AII phase. The AII phase content in the prepared composite phase gypsum powder is 12±3%, and the DH phase content is less than 1.0%.
[0065] (3) Impingement flow cooling and modification stage: The high-temperature composite phase gypsum powder from the calcining fluidized bed 6 passes through the 45 mm feed nozzle 805 and enters the impingement chamber 807 of the impingement flow cooler 8 at a flow rate of 8 m / s. At the same time, the cooling air passes through the 32 mm air inlet nozzle 806 and enters the impingement chamber 807 at a flow rate of 15 m / s. The impact forms a large contact area and high turbulence and reaches a high relative velocity between phases, which strengthens the heat transfer of the high-temperature composite phase gypsum powder and accelerates the cooling rate of the high-temperature composite phase gypsum powder. The temperature of the composite phase gypsum powder is reduced to 95°C in a short time, and then enters the cyclone cooler 9. After cyclone cooling, the temperature of the composite phase gypsum powder is further reduced to 52°C. Finally, it enters the ball mill 10 for ball milling modification to a particle size distribution range of 38 to 75 μm. The modified composite phase gypsum powder enters the buffer bin 14.
[0066] (4) Rapid aging stage: The compressed air generated by the air compressor 19 enters the gas humidification tank 18 through the gas control cabinet, and the humidified gas with a relative humidity of 95% enters the gas mixing tank 17. At the same time, the hot gas with a temperature of 44°C and a relative humidity of 26% coming out of the cyclone cooler 9 also enters the gas mixing tank 17 from another air inlet of the gas mixing tank. The volume flow ratio of the humidified gas to the hot gas is 5.5:1, and the temperature of the formed mixed gas is 30°C and the relative humidity is 84%. The mixed gas enters from the bottom of the aging fluidized bed 15 after passing through the gas control cabinet, and is used as fluidizing air after passing through the air distribution plate, with a gas velocity of 1.0 m / s. The composite phase gypsum powder in the buffer bin 14 continuously enters the fluidized bed from the left chamber feed port of the aging fluidized bed 15. Under the action of the fluidizing wind, the composite phase gypsum powder is in a fluidized state. The AIII phase in the composite phase gypsum powder absorbs the gaseous water in the binary mixed gas and transforms into the HH phase. After 130 minutes of aging, the fluidization height of the composite phase gypsum powder reaches the designed height of the right chamber discharge port, and the composite phase gypsum powder is continuously discharged into the finished product bin 20. The tail gas generated by the aging fluidized bed 15 enters the first bag dust removal stage 12.
[0067] The test results of the phase components of the composite phase gypsum powder prepared by the above process are shown in the following table, which meets the requirements of the target phase component control.
[0068] Test items Phase AIII Adherent water AII phase DH phase HH phase result / % 0.33 0 14.6 0.82 78.5
[0069] Example 4
[0070] The composite phase gypsum was prepared by using the device in Example 1. The treatment object in this example was phosphogypsum after water washing and purification in a chemical plant. The analysis results are as follows.
[0071] Test items Adherent water Crystal water grade pH result / % 23 19.7 91 5.8
[0072] The target phase components of the composite phase gypsum powder prepared from phosphogypsum are shown in the following table.
[0073] Test items Phase AIII / adherent water AII phase DH phase HH phase result / % <1% 80±3% <1.5% 10±3%
[0074] (1) Raw material pretreatment stage: During the storage period, the phosphogypsum raw materials are intermittently turned by a grab bucket to reduce the free water content of the phosphogypsum to 7.5%. The homogenized phosphogypsum passes through a vibrating screening device 1 with a square screen with a side length of 2.5 cm. The phosphogypsum under the screen enters the lower end of the Venturi dryer 4 through a metering screw feeder 2.
[0075] (2) Fluidized graded calcination stage: The hot flue gas of 165°C provided by the coal-fired hot blast furnace 3 enters from the lower end of the venturi dryer 4 at a flow rate of 17 m / s. After being accelerated, the hot air breaks up the agglomerated phosphogypsum and removes the free water of the phosphogypsum. It is blown out from the upper end in the form of gas-solid fluid and enters the cyclone separator 5. The high-humidity gas enters the first bag filter 12 from the top outlet of the cyclone separator 5. The phosphogypsum powder coming out of the bottom enters from the feed port on the left chamber of the calcination fluidized bed 6. The hot air generated by the natural gas hot blast furnace 7 enters from the two air inlets at the bottom of the calcination fluidized bed 6 and passes through the air distribution plate at a flow rate of 1.7 m / s to fluidize the phosphogypsum powder. The phosphogypsum powder in the left chamber enters the right chamber from the bottom connection, and the material level height tends to be consistent under the action of the fluidizing air. As the phosphogypsum powder continuously enters the left chamber, the material level in the right chamber also rises. When the material level reaches the height of the upper discharge port of the right chamber, the calcined composite phase gypsum powder is continuously discharged. During the fluidized calcination process of the phosphogypsum powder, the material temperature is controlled at 425±5℃, the pneumatic valve opening is 85%, and the residence time is 80±3min. The DH phase in the phosphogypsum powder gradually transforms into the HH phase, AIII phase and AII phase. The AII phase content in the prepared composite phase gypsum powder is 80% and the DH phase content is less than 1.0%.
[0076] (3) Impingement flow cooling and modification stage: The high-temperature composite phase gypsum powder from the calcining fluidized bed 6 passes through the 30 mm feed nozzle 805 and then enters the impingement chamber 807 of the impingement flow cooler 8 at a flow rate of 12 m / s. At the same time, the cooling air passes through the 21 mm air inlet nozzle 806 and then enters the impingement chamber 807 at a flow rate of 19 m / s. The impact forms a large contact area and high turbulence and reaches a high relative velocity between phases, which strengthens the heat transfer of the high-temperature composite phase gypsum powder and accelerates the cooling rate of the high-temperature composite phase gypsum powder. The temperature of the composite phase gypsum powder is reduced to 125°C in a short time, and then enters the cyclone cooler 9. After cyclone cooling, the temperature of the composite phase gypsum powder is further reduced to 65°C. Finally, it enters the ball mill 10 for ball milling modification to a particle size distribution range of 38 to 75 μm. The modified composite phase gypsum powder enters the buffer bin 14.
[0077] (4) Rapid aging stage: The compressed air generated by the air compressor 19 enters the gas humidification tank 18 through the gas control cabinet, and the humidified gas with a relative humidity of 95% enters the gas mixing tank 17. At the same time, the hot gas with a temperature of 60°C and a relative humidity of 10% coming out of the cyclone cooler 9 also enters the gas mixing tank 17 from another air inlet of the gas mixing tank. The volume flow ratio of the humidified gas to the hot gas is 2:1, and the temperature of the formed mixed gas is 50°C and the relative humidity is 65%. The mixed gas enters from the bottom of the aging fluidized bed 15 after passing through the gas control cabinet, and is used as fluidizing air after passing through the air distribution plate, with a gas velocity of 2.6m / s. The composite phase gypsum powder in the buffer bin 14 continuously enters the fluidized bed from the left chamber feed port of the aging fluidized bed 15. Under the action of the fluidizing wind, the composite phase gypsum powder is in a fluidized state. The AIII phase in the composite phase gypsum powder absorbs the gaseous water in the binary mixed gas and transforms into the HH phase. After 60 minutes of aging, the fluidization height of the composite phase gypsum powder reaches the designed height of the right chamber discharge port, and the composite phase gypsum powder is continuously discharged into the finished product bin 20. The tail gas generated by the aging fluidized bed 15 enters the first bag dust removal stage 12.
[0078] The test results of the phase components of the composite phase gypsum powder prepared by the above process are shown in the following table, which meets the requirements of the target phase component control.
[0079] Test items Phase AIII Adherent water AII phase DH phase HH phase result / % 0 0.41 79.2 0.29 9.5
[0080] Although the present invention is described herein with reference to a number of illustrative embodiments of the present invention, it will be appreciated that those skilled in the art may devise numerous other modifications and implementations that will fall within the scope and spirit of the principles disclosed herein. More specifically, within the scope of the present disclosure, drawings, and claims, a variety of variations and modifications may be made to the components or layout. In addition to variations and modifications made to the components or layout, other uses will also be apparent to those skilled in the art.
Claims
1. A method for preparing composite phase gypsum with adjustable phase components from phosphogypsum, characterized in that The steps include: S1. The phosphogypsum raw material with a free water content of less than 6% is screened by a vibrating screening device (1), and the screened phosphogypsum enters a venturi dryer (4) through a metering screw feeder (2), and enters a cyclone separator (5) after drying. The separated phosphogypsum powder enters a calcining fluidized bed (6); S2. The phosphogypsum powder enters the left chamber from the feed port of the calcining fluidized bed (6), and the hot air enters from the bottom of the calcining fluidized bed (6). The phosphogypsum powder contacts the hot air at a flow rate of 0.5 to 5 m / s and enters the right chamber from the connection point at the bottom of the left chamber in a fluidized state, and is finally discharged from the upper discharge port of the right chamber. The calcination temperature of the fluidized phosphogypsum powder is controlled to be 300 to 450° C., and the residence time in the calcining fluidized bed (6) is 30 to 90 min, thereby preparing a high-temperature composite phase gypsum powder; S3. The high-temperature composite phase gypsum powder enters the impinging flow cooler (8) at a flow rate of 8 to 12 m / s, collides with the cooling air at a flow rate of 14 to 20 m / s to cool it, and then enters the cyclone cooler (9) to further cool the composite phase gypsum powder to below 70° C. The hot air after heat exchange in the cyclone cooler is dedusted by the second bag dust collector (12); S4. After cooling, the composite phase gypsum powder enters the ball mill (10) to modify the appearance and particle size of the composite phase gypsum powder particles by ball milling, and the particle size distribution range after modification is controlled to be 38 to 75 μm. The modified composite phase gypsum powder is sent to the buffer bin (14) for temporary storage; S5. After the compressed air is humidified, it is mixed with the hot air after dust removal by the second bag filter (12) in the gas mixing tank (17) to obtain a mixed gas with a temperature of 25-60°C and a relative humidity of 40-90%. The mixed gas is fed into the aging fluidized bed (15) from the bottom. The composite phase gypsum powder in the buffer bin (14) enters from the feed port of the left chamber of the aging fluidized bed (15), contacts with the mixed gas with a flow rate of 0.5-3 m / s and is in a fluidized state. Since the bottom of the left chamber is connected to the bottom of the right chamber, the composite phase gypsum powder enters the right chamber from the connection, and is finally discharged from the upper discharge port of the right chamber to the finished product bin (20). The composite phase gypsum powder in the fluidized state is controlled to stay in the aging fluidized bed (15) for 50-150 minutes to obtain a composite phase gypsum finished product. The tail gas of the aging fluidized bed (15) enters the first bag filter (12).
2. The method according to claim 1, characterized in that: In step S1, the calcium sulfate dihydrate content in the phosphogypsum raw material is ≥85%, the pH value is ≥3.0, and the pile is turned intermittently with a grab bucket before screening; the vibration screening equipment (1) has a sieve hole diameter of ≤3cm.
3. The method according to claim 1, characterized in that: In step S1, hot air with a temperature of 150-200° C. and a gas velocity of 15-20 m / s is introduced from the bottom of the Venturi dryer (4), and the hot air is provided by a coal-fired hot air furnace (3); the tail gas of the cyclone separator (5) is sent to the first bag dust collector (12).
4. The method according to claim 1, characterized in that: The hot air in step S2 is provided by a natural gas hot air furnace (7).
5. The method according to claim 1, characterized in that: The cooling air in step S3 is provided by a fan (11), and the cooling air is natural wind.
6. The method according to claim 1, characterized in that: The calcining fluidized bed (6) and the aging fluidized bed (15) are both provided with pneumatic valves (21) at their discharge ports. During the production process, the opening of the pneumatic valves (21) is 50-100%.
7. The method according to claim 1, characterized in that: The composite phase gypsum product has an AII phase content of 10-90%, an HH phase content of 5-85%, a DH phase content of 0.5-1.5%, an AIII phase content of 0-0.5%, and an attached water content of 0-1.0%.
8. The method according to any one of claims 1 to 7, characterized in that: The device used in the method comprises a vibrating screening machine (1), a metering screw feeder (2), a venturi dryer (4), a cyclone separator (5), a calcining fluidized bed (6), an impinging flow cooler (8), a cyclone cooler (9), a ball mill (10), a buffer bin (14), an aging fluidized bed (15), and a finished product bin (20) which are connected in sequence; the air inlet of the venturi dryer (4) is connected to the air outlet of the coal-fired hot air furnace (3), and the air outlet of the cyclone separator (5) is connected to the air inlet of the first bag dust collector (12); the exhaust port at the top of the calcining fluidized bed (6) is connected to the air inlet of the natural gas hot air furnace (7) through an exhaust gas pipeline. The air inlet of the impinging flow cooler (8) is connected to the air outlet of the natural gas hot blast furnace (7); the air inlet of the impinging flow cooler (8) is connected to the fan (11), the discharge port of the impinging flow cooler (8) is connected to the feed port of the cyclone cooler (9), and the air outlet of the cyclone cooler (9) is connected to the air inlet of the gas mixing tank (17) via the second bag filter (13); the top exhaust port of the aging fluidized bed (15) is connected to the first bag filter (12) via the tail gas pipeline, and the bottom air inlet is connected to the air outlet of the gas mixing tank (17); the air inlet of the gas mixing tank (17) is connected to the gas humidification tank (18) and the air compressor (19) in sequence.
9. The method according to claim 8, characterized in that: The impinging flow cooler (8) comprises an upper separation chamber (804) and a lower impinging chamber (807); the separation chamber (804) and the impinging chamber (807) are connected; a feed nozzle (805) and an air intake nozzle (806) are arranged on opposite sides of the impinging chamber (807); a discharge port (808) is arranged at the bottom of the impinging chamber (807); an exhaust port (801) is arranged at the top of the separation chamber (804); and the exhaust port (801) is connected to the air intake of the coal-fired hot air furnace (3) through a dust separation device (22).
10. The method according to claim 9, characterized in that: The diameter of the pipe at the connection between the separation chamber (804) and the impact chamber (807) is 1 / 10 to 1 / 20 of the inner diameter of the impact chamber (807).