A polylactic acid-Ulva prolifera polysaccharide grafted sealing agent, its preparation method and application

The preparation of the plugging agent by esterification reaction of polylactic acid-Ulva prolifera polysaccharide grafted plugging agent solves the problems of self-cleaning of drilling fluid plugging agent and reservoir damage, realizes self-degradation and porosity increase, and improves drilling fluid production.

CN118852638BActive Publication Date: 2026-11-10CHINA PETROLEUM & CHEMICAL CORP +3
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310477518.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2026-11-10
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Existing drilling fluid plugging agents require subsequent removal operations, which can easily cause secondary damage to the reservoir, and the degradation time is difficult to control.

Method used

A polylactic acid-Ulva prolifera polysaccharide grafted plugging agent is used. Polylactic acid and Ulva prolifera polysaccharide are grafted through an esterification reaction to form a self-degradable plugging agent. It degrades on its own after drilling, avoiding subsequent removal operations. During degradation, it reacts with the formation rock to increase the pore size.

Benefits of technology

It achieves self-removal of the plugging agent, reduces secondary damage to the reservoir, increases fluid production, and increases pore volume through degradation, thereby improving the later fluid production effect.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention proposes a polylactic acid-Ulva prolifera polysaccharide grafted plugging agent, its preparation method, and its application. The plugging agent, by mass percentage, comprises 50%–80% low-molecule polylactic acid, 15%–45% Ulva prolifera polysaccharide, 3%–5% esterifying agent, and the remainder being water. This plugging agent self-degrades after drilling operations, depending on the timing of subsequent well completion operations. The plugging agent material does not damage the reservoir and eliminates the need for secondary fracturing or other post-operational removal and plugging procedures. Furthermore, the plugging agent exhibits acidic degradation properties, allowing it to react with the rocks in the formation, increasing pore size and thus improving fluid production in subsequent operations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of drilling plugging technology, specifically relating to a polylactic acid-Ulva prolifera polysaccharide grafted plugging agent, its preparation method, and its application. Background Technology

[0002] During drilling, water and solid particles in the drilling fluid can seep into the formation through formation pores. Especially when encountering reservoirs, the migration of solid particles causing formation blockage and the water-locking effect caused by liquid intrusion are the main reasons for reservoir damage and reduced production. Currently, the common method is to add plugging agents to the drilling fluid to seal the formation and prevent harmful solid and liquid phases from intruding and damaging it. Plugging agents are generally divided into two types: hard plugging and soft plugging. Hard plugging uses rigid particles of different sizes based on the distribution of formation pores to create a hard seal, while soft plugging refers to the treatment agent forming a soft sealing film on the wellbore surface to prevent solid and liquid phases from intruding into the formation. Most plugging agents currently used require post-well completion removal operations; incomplete removal can cause secondary damage to the reservoir.

[0003] In the patent (CN 108384520A) applied for by Zhang Jie et al. in China, a biodegradable fiber plugging agent for drilling fluid and its preparation method are prepared by copolymerizing fiber and other materials with polylactic acid. Due to the grafting of fibers, the degradation time is increased and the degradation difficulty is increased.

[0004] Therefore, there is an urgent need to develop a self-cleaning plugging agent that does not require subsequent operations, has an ideal cleaning effect, and will not cause secondary pollution to the reservoir. Summary of the Invention

[0005] To address the aforementioned problems in the prior art, this invention proposes a polylactic acid-Ulva prolifera polysaccharide grafting and sealing agent, its preparation method, and its application.

[0006] In a first aspect, the present invention proposes a polylactic acid-Ulva prolifera polysaccharide grafting and sealing agent, the components of which, by mass percentage, include 50% to 80% small molecule polylactic acid, 15% to 45% Ulva prolifera polysaccharide, 3% to 5% esterifying agent, and the remainder being water.

[0007] It should be noted that polylactic acid (PLA) and its copolymers are synthetic polymers with excellent biocompatibility and biodegradability. They are non-toxic, non-irritating, high-strength, highly malleable, and easy to process, and therefore have been widely used in biodegradable fibers and biodegradable plastic products.

[0008] Ulva prolifera polysaccharide is a polysaccharide extracted from Ulva prolifera. Ulva prolifera is an aquatic plant that grows widely in coastal areas. Extracting Ulva prolifera polysaccharide from Ulva prolifera is a low-cost process, and the product is environmentally friendly and easily degradable.

[0009] Polylactic acid (PLA) and *Ulva prolifera* polysaccharide are grafted together via esterification. Through a well-controlled process, the degradation time of the product can be managed. After drilling, the plugging agent self-degrades according to the timing of subsequent well completion operations. The plugging agent does not damage the reservoir and eliminates the need for secondary fracturing or other post-completion removal operations. Furthermore, the plugging agent degrades to an acidic state, reacting with the rock in the formation to increase pore size and improve fluid production in later operations.

[0010] As a specific embodiment of the present invention, the molecular weight of the small molecule polylactic acid is between 30,000 and 80,000.

[0011] As a specific embodiment of the present invention, the small molecule polylactic acid is polylactic acid powder, polylactic acid microspheres, or polylactic acid emulsion.

[0012] As a specific embodiment of the present invention, the small molecule polylactic acid is polylactic acid powder with a particle size range of 300 mesh to 500 mesh.

[0013] As a specific embodiment of the present invention, the polylactic acid microspheres are polylactic acid microspheres prepared by reverse emulsion polymerization, and their particle size ranges from 1 μm to 100 μm.

[0014] As a specific embodiment of the present invention, the polylactic acid emulsion solvent is one or a mixture of several of dichloromethane, chloroform, and acetone.

[0015] As a specific embodiment of the present invention, the preparation process of the *Ulva prolifera* polysaccharide includes the following steps:

[0016] The defatted Ulva lactuca powder was extracted with hot water, cooled, and the pH was adjusted to 5.5. Papain (8% by mass) was added to remove the protein, followed by ethanol precipitation. The extraction was performed with water or ethanol.

[0017] As a specific embodiment of the present invention, the esterifying agent is at least one of oxalic acid, malonic acid, succinic acid, and adipic acid.

[0018] In a second aspect, the present invention provides a method for preparing the polylactic acid-Ulva prolifera polysaccharide grafted sealing agent as described in the first aspect, comprising the following steps:

[0019] S1: Mix small molecule polylactic acid with a solvent to obtain a dispersed polylactic acid dispersion;

[0020] S2: Mix the polylactic acid dispersion obtained in step S1 with the Ulva prolifera polysaccharide to obtain a polylactic acid-Ulva prolifera polysaccharide mixed solution;

[0021] S3: The polylactic acid-Ulva prolifera polysaccharide mixed solution obtained in step S2 is subjected to esterification reaction with an esterifying agent under the action of a catalyst to obtain polylactic acid-Ulva prolifera polysaccharide graft.

[0022] S4: Dry and granulate the polylactic acid-Ulva prolifera polysaccharide graft obtained in step S3 to obtain polylactic acid-Ulva prolifera polysaccharide graft sealing agent.

[0023] In a specific embodiment of the present invention, in step S1, the mass-to-volume ratio of the small molecule polylactic acid to the solvent is 1g:2.5ml to 7ml; the solvent is one of water, dichloromethane, chloroform, and acetone.

[0024] As a specific embodiment of the present invention, in step S2, the mass ratio of the small molecule polylactic acid to the seaweed polysaccharide is (1-6):1; the conditions for mixing the polylactic acid dispersion and the seaweed polysaccharide include: a mixing temperature of 70℃~90℃ and a stirring rate of 50-300 rpm.

[0025] In a specific embodiment of the present invention, in step S3, the esterification reaction temperature is 150℃~180℃; the catalyst is at least one of macroporous strong acid styrene-based cation exchange resin and macroporous strong acid acrylic-based cation exchange resin.

[0026] For example, the esterification reaction is carried out in a tubular reactor with a catalyst, and a continuous esterification experiment is conducted. The esterification agent vapor enters from the bottom of the reactor at a bed temperature of 100°C to 120°C and a vessel temperature of 150°C to 180°C, while the polylactic acid-Ulva prolifera polysaccharide mixed solution prepared in step S3 is continuously fed from the top of the reactor. The two react in opposite directions in the catalyst section of the reactor to carry out the esterification reaction, and the continuous esterification product enters the bottom of the vessel connected to the reactor.

[0027] Thirdly, the present invention provides the application of the polylactic acid-Ulva prolifera polysaccharide grafted plugging agent described in the first aspect or the polylactic acid-Ulva prolifera polysaccharide grafted plugging agent prepared by the preparation method described in the second aspect in the field of well plugging.

[0028] All of the above-mentioned raw materials used in this invention can be prepared in-house or purchased commercially; this invention does not impose any particular limitations on them.

[0029] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0030] 1. The polylactic acid-Ulva prolifera polysaccharide grafted plugging agent of the present invention is a plugging agent that can achieve self-degradation and self-removal, which solves the problems of the prior art where the plugging agent needs to be removed in the later stage or the removal is incomplete and causes secondary damage to the reservoir.

[0031] 2. The polylactic acid-Ulva prolifera polysaccharide grafting and sealing agent of the present invention, after self-degradation, can also increase the pore volume due to its acidity, thereby improving the liquid production. Detailed Implementation

[0032] The present invention will be further described below with reference to specific embodiments, but this does not constitute any limitation on the present invention.

[0033] In the various embodiments of the present invention, the *Ulva prolifera* polysaccharide was prepared by the following method:

[0034] The defatted seaweed powder was extracted with hot water, cooled, and the pH was adjusted to 5.5. After adding 8% papain to remove the protein, it was precipitated with ethanol.

[0035] In the various embodiments of the present invention, the catalyst is a macroporous, strongly acidic styrene-based cation exchange resin.

[0036] Example 1

[0037] This embodiment provides a polylactic acid-Ulva prolifera polysaccharide grafted sealing agent and its preparation method, the details of which are as follows:

[0038] S1: Weigh 2000g of small molecule polylactic acid powder with a molecular weight of 60000 and a particle size of 500 mesh, add it to 5000ml of dichloromethane, and stir thoroughly until all polylactic acid particles are dissolved.

[0039] S2: Heat the polylactic acid dispersion prepared in S1 to 70°C, slowly add 1500g of Ulva prolifera polysaccharide and stir until the Ulva prolifera polysaccharide is completely dissolved to form a polylactic acid-Ulva prolifera polysaccharide mixed solution.

[0040] S3: A catalyst is loaded into a tubular reactor for continuous esterification experiments. Oxalic acid vapor enters from the bottom of the reactor at a bed temperature of 100°C and a vessel temperature of 150°C. The polylactic acid-Ulva prolifera polysaccharide mixed solution prepared in S2 is continuously fed from the top of the reactor. The two react in opposite directions in the catalyst section of the reactor to carry out the esterification reaction. The continuous esterification product enters the bottom of the vessel connected to the reactor.

[0041] S4: The product from the bottom of the reactor in S3 is dried, extruded, and granulated to obtain polylactic acid-Ulva prolifera polysaccharide grafting and sealing agent.

[0042] The raw material components for preparing the polylactic acid-Ulva prolifera polysaccharide grafting and sealing agent in Example 1, by mass percentage, are: 56% small molecule polylactic acid, 42% Ulva prolifera polysaccharide, 0.5% esterifying agent, and the remainder is water.

[0043] Example 2

[0044] This embodiment provides a polylactic acid-Ulva prolifera polysaccharide grafted sealing agent and its preparation method, the details of which are as follows:

[0045] S1: Weigh 2300g of small molecule polylactic acid emulsion, wherein the number average molecular weight of the small molecule polylactic acid is 60000 and the particle size is 300 mesh, add it to 7000g of deionized water, and stir thoroughly until the polylactic acid particles are completely dispersed.

[0046] S2: Heat the polylactic acid dispersion prepared in step S1 to 80°C, and slowly add 1200g of Ulva prolifera polysaccharide while stirring until the Ulva prolifera polysaccharide is completely dissolved.

[0047] S3: A catalyst is loaded into a tubular reactor for continuous esterification experiments. Oxalic acid vapor enters from the bottom of the reactor at a bed temperature of 110°C and a vessel temperature of 170°C. The polylactic acid-Ulva prolifera polysaccharide mixed solution prepared in step S2 is continuously fed from the top of the reactor. The two react in opposite directions in the catalyst section of the reactor to carry out the esterification reaction. The continuous esterification product enters the bottom of the vessel connected to the reactor.

[0048] S4: The product from the bottom of the reactor in step S3 is dried, extruded, and granulated to obtain polylactic acid-Ulva prolifera polysaccharide grafting and sealing agent.

[0049] The raw materials used to prepare the polylactic acid-Ulva prolifera polysaccharide grafting and sealing agent in Example 2, by mass percentage, are: 62% low-molecular-weight polylactic acid, 35% Ulva prolifera polysaccharide, 0.6% esterifying agent, and the remainder is water.

[0050] Example 3

[0051] This embodiment provides a polylactic acid-Ulva prolifera polysaccharide grafted sealing agent and its preparation method, the details of which are as follows:

[0052] S1: Weigh 2500g of small molecule polylactic acid microspheres. The number average molecular weight of the polylactic acid microspheres is 40000 and the median particle size is 75μm. Add them to 10000g of deionized water and stir thoroughly until the polylactic acid particles are completely dispersed.

[0053] S2: Heat the polylactic acid dispersion prepared in step S1 to 90°C, slowly add 1000g of Ulva prolifera polysaccharide and stir until the Ulva prolifera polysaccharide is completely dissolved to form a polylactic acid-Ulva prolifera polysaccharide mixed solution.

[0054] S3: A catalyst is loaded into a tubular reactor for continuous esterification experiments. Oxalic acid vapor enters from the bottom of the reactor at a bed temperature of 115°C and a vessel temperature of 160°C. The polylactic acid-Ulva prolifera polysaccharide mixed solution prepared in step S2 is continuously fed from the top of the reactor. The two react in opposite directions in the catalyst section of the reactor to carry out the esterification reaction. The continuous esterification product enters the bottom of the vessel connected to the reactor.

[0055] S4: The product from the bottom of the reactor in step S3 is dried, extruded, and granulated to obtain polylactic acid-Ulva prolifera polysaccharide grafting and sealing agent.

[0056] Example 3: The raw materials for preparing the polylactic acid-Ulva prolifera polysaccharide grafted plugging agent, by mass percentage, are: 67% low-molecular-weight polylactic acid, 30% Ulva prolifera polysaccharide, 0.5% esterifying agent, and the remainder is water.

[0057] Example 4

[0058] This embodiment provides a polylactic acid-Ulva prolifera polysaccharide grafted sealing agent and its preparation method, the details of which are as follows:

[0059] S1: Weigh 2900g of small molecule polylactic acid emulsion, wherein the number average molecular weight of the small molecule polylactic acid is 50000 and the particle size is 500 mesh, add it to 10000g of deionized water, and stir thoroughly until the polylactic acid particles are completely dispersed.

[0060] S2: Heat the polylactic acid dispersion prepared in step S1 to 90°C, slowly add 600g of Ulva prolifera polysaccharide and stir until the Ulva prolifera polysaccharide is completely dissolved to form a polylactic acid-Ulva prolifera polysaccharide mixed solution.

[0061] S3: A catalyst is loaded into a tubular reactor for continuous esterification experiments. Oxalic acid vapor enters from the bottom of the reactor at a bed temperature of 120°C and a vessel temperature of 180°C. The polylactic acid-Ulva prolifera polysaccharide mixed solution prepared in step S2 is continuously fed from the top of the reactor. The two react in opposite directions in the catalyst section of the reactor to carry out the esterification reaction. The continuous esterification product enters the bottom of the vessel connected to the reactor.

[0062] S4: The product from the bottom of the reactor in step S3 is dried, extruded, and granulated to obtain polylactic acid-Ulva prolifera polysaccharide grafting and sealing agent.

[0063] Example 4: The raw materials for preparing the polylactic acid-Ulva prolifera polysaccharide grafted plugging agent, by mass percentage, are: 76.5% low molecular weight polylactic acid, 20% Ulva prolifera polysaccharide, 0.6% esterifying agent, and the remainder is water.

[0064] Test Example 1

[0065] Filtration loss reduction performance test

[0066] The degradation properties of the synthesized polylactic acid-Ulva prolifera polysaccharide grafted plugging agent were evaluated. Simultaneously, 12g of the polylactic acid-Ulva prolifera polysaccharide grafted plugging agent was added to 400ml of a 6% sodium bentonite slurry to evaluate its effect on the slurry filtration loss. The experimental results are shown in Table 1.

[0067] Table 1 Performance Evaluation of Polylactic Acid-Ulva Propionibacterium Grafted Plugging Agent

[0068] Filtration loss / ml 10-day degradation rate / % 15-day degradation rate / % 20-day degradation rate / % base slurry 25 Example 1 10.2 57.2 87.9 100 Example 2 12.6 69.3 100 100 Example 3 12.5 93.2 100 100 Example 4 10.0 56.2 78.8 89.1

[0069] Experimental data show that this plugging agent has good degradation performance, and its degradation time can be controlled by adjusting the synthesis process within a certain range. Simultaneously, this plugging agent can effectively reduce drilling fluid filtrate loss, further minimizing the damage of the filtrate to the reservoir.

[0070] Example 5

[0071] The degradation of polylactic acid powder was evaluated, and 12g of polylactic acid-Ulva polysaccharide grafting and sealing agent was added to 400ml of 6% sodium bentonite slurry to evaluate its effect on the filtrate loss of the slurry.

[0072] Example 6

[0073] The degradation of polylactic acid microspheres was evaluated, and the effect of adding 12g of polylactic acid-Ulva polysaccharide grafting and sealing agent to 400ml of 6% sodium bentonite slurry on the filtration loss of the slurry was evaluated.

[0074] Example 7

[0075] The degradation of polylactic acid microemulsion was evaluated. At the same time, 12g of polylactic acid-Ulva polysaccharide grafting and sealing agent was added to 400ml of 6% sodium bentonite slurry to evaluate its effect on the filtration loss of the base slurry.

[0076] The experimental results are shown in Table 2.

[0077] Table 1 Performance Evaluation of Polylactic Acid-Ulva Propionibacterium Grafted Plugging Agent

[0078] 10-day degradation rate / % 15-day degradation rate / % 20-day degradation rate / % Example 5 10.3 16.2 25.4 Example 6 45.2 78.3 100 Example 7 2.5 3.1 5.2

[0079] Test Example 2

[0080] Leak-sealing performance test

[0081] (1) Grind the product of Example 1 to a particle size of 200 mesh, the product of Example 2 to 250 mesh, the product of Example 3 to 200-250 mesh, and the product of Example 4 to 350-400 mesh. Take products of different particle sizes and mix them in the following mass ratio to form a biodegradable sealing agent: Example 1: Example 2: Example 3: Example 4 = 1:1:2:2.

[0082] (2) A 6% sodium bentonite slurry was prepared as the base mud, and a 3% biodegradable plugging agent was added to the mud for core plugging tests. The core permeability before plugging was 261.2 mD, and the core permeability after plugging was 31.5 mD, with a core plugging rate of 87.9%. It can be seen that the plugging agent has a significant plugging effect.

[0083] In summary, the polylactic acid-Ulva prolifera polysaccharide grafted plugging agent of this invention uses biodegradable and environmentally friendly polylactic acid and Ulva prolifera polysaccharide to synthesize a self-degradable plugging agent. Extracting Ulva prolifera polysaccharide from Ulva prolifera is inexpensive, and the product is environmentally friendly and easily degradable. By grafting polylactic acid and Ulva prolifera polysaccharide together through an esterification reaction, the degradation time of the product can be controlled through a reasonable process. After drilling operations, the plugging agent can self-degrade according to the timing of subsequent well completion operations. The plugging agent material will not damage the reservoir and does not require secondary fracturing or other subsequent removal and plugging operations. Furthermore, the plugging agent exhibits acidity during degradation, which allows it to react with the rocks in the formation, increasing the pore size and thereby improving the fluid production rate in subsequent operations.

[0084] Any numerical value mentioned in this invention, if there is only a two-unit interval between any minimum and any maximum value, includes all values ​​that increase by one unit each time from the minimum to the maximum value. For example, if the amount of a component, or the value of a process variable such as temperature, pressure, or time, is stated as 50-90, in this specification it means specifically listing values ​​such as 51-89, 52-88… and 69-71 and 70-71, etc. For non-integer values, it may be appropriately considered that a unit is 0.1, 0.01, 0.001, or 0.0001. These are merely some specifically specified examples. In this application, in a similar manner, all possible combinations of numerical values ​​between the listed minimum and maximum values ​​are considered to have been disclosed.

[0085] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.

Claims

1. A polylactic acid-Ulva prolifera polysaccharide grafted sealing agent, characterized in that, The raw materials, by mass percentage, include 50%~80% small molecule polylactic acid, 15%~45% Ulva polysaccharide, 0.5%~5% esterifying agent, and the remainder is water. The small molecule polylactic acid is polylactic acid microspheres, which are prepared by reverse emulsion polymerization. The particle size range of the polylactic acid microspheres is 1μm~100μm, and the number average molecular weight of the polylactic acid microspheres is 30,000-40,000. The method for preparing the plugging agent includes the following steps: S1: Mix small molecule polylactic acid with a solvent to obtain a dispersed polylactic acid dispersion; S2: Mix the polylactic acid dispersion obtained in step S1 with the Ulva prolifera polysaccharide to obtain a polylactic acid-Ulva prolifera polysaccharide mixed solution; S3: The polylactic acid-Ulva prolifera polysaccharide mixed solution obtained in step S2 is subjected to an esterification reaction with an esterifying agent under the action of a catalyst to obtain a polylactic acid-Ulva prolifera polysaccharide graft; the esterification reaction is a counter-contact reaction between the esterifying agent vapor and the polylactic acid-Ulva prolifera polysaccharide mixed solution in the catalyst section of a tubular reactor; S4: Dry and granulate the polylactic acid-Ulva prolifera polysaccharide graft obtained in step S3 to obtain polylactic acid-Ulva prolifera polysaccharide grafted sealing agent; The catalyst is at least one of macroporous strong acid styrene-based cation exchange resin and macroporous strong acid acrylic-based cation exchange resin.

2. The sealing agent according to claim 1, characterized in that, The preparation method of the *Ulva prolifera* polysaccharide includes: extracting defatted *Ulva prolifera* powder, cooling, adding papain to remove protein, and then precipitating with ethanol.

3. The sealing agent according to claim 2, characterized in that, The extraction temperature is 30-60℃; the pH value is adjusted to 5-6 after extraction; the amount of papain added is 6-10% of the mass of the dried seaweed powder.

4. The sealing agent according to claim 3, characterized in that, The pH value is adjusted to 5.5 after extraction, and / or the amount of papain added is 8% of the mass of the dried seaweed powder.

5. The sealing agent according to any one of claims 1-4, characterized in that, The esterifying agent is at least one of oxalic acid, malonic acid, succinic acid, and adipic acid.

6. A method for preparing the polylactic acid-Ulva prolifera polysaccharide grafted sealing agent according to any one of claims 1-5, characterized in that, Includes the following steps: S1: Mix small molecule polylactic acid with a solvent to obtain a dispersed polylactic acid dispersion; S2: Mix the polylactic acid dispersion obtained in step S1 with the Ulva prolifera polysaccharide to obtain a polylactic acid-Ulva prolifera polysaccharide mixed solution; S3: The polylactic acid-Ulva prolifera polysaccharide mixed solution obtained in step S2 is subjected to an esterification reaction with an esterifying agent under the action of a catalyst to obtain a polylactic acid-Ulva prolifera polysaccharide graft; the esterification reaction is a counter-contact reaction between the esterifying agent vapor and the polylactic acid-Ulva prolifera polysaccharide mixed solution in the catalyst section of a tubular reactor; S4: Dry and granulate the polylactic acid-Ulva prolifera polysaccharide graft obtained in step S3 to obtain polylactic acid-Ulva prolifera polysaccharide grafted sealing agent; The catalyst is at least one of macroporous strong acid styrene-based cation exchange resin and macroporous strong acid acrylic-based cation exchange resin.

7. The preparation method according to claim 6, characterized in that, In step S1, the mass-to-volume ratio of the small molecule polylactic acid to the solvent is 1g: 2.5ml~7ml; the solvent is one of water, dichloromethane, chloroform, and acetone.

8. The preparation method according to claim 6 or 7, characterized in that, In step S2, the mass ratio of the small molecule polylactic acid to the Ulva prolifera polysaccharide is (1-6):1; the conditions for mixing the polylactic acid dispersion with the Ulva prolifera polysaccharide include: a mixing temperature of 70℃~90℃ and a stirring speed of 50-300rpm. And / or, in step S3, the esterification reaction temperature is 150℃~180℃.

9. The application of the polylactic acid-Ulva prolifera polysaccharide grafted plugging agent according to any one of claims 1-5 or the polylactic acid-Ulva prolifera polysaccharide grafted plugging agent prepared by the preparation method according to any one of claims 6-8 in the field of well plugging.

Citation Information

Patent Citations

  • Degradable fiber blocking agent for drilling fluid and preparation method thereof

    CN108384520A

  • Polylactic acid-enteromorpha polysaccharide grafted plugging agent and preparation method thereof

    CN113549435A