Silk fabric sensor, preparation method thereof and application of silk fabric sensor in muscle stress-strain detection and human body biomolecule detection
Through the combination of silk fiber membrane with silver nanoparticles and gold seed layer, the stability problem of the flexible sensor under the influence of external deformation and environmental factors is solved, and high stability and sensitivity detection results are achieved, which is suitable for muscle stress and biomolecules. detection.
Patent Information
- Application Number
- CN202410908341.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-29
AI Technical Summary
Existing flexible sensors have challenges in multi-functional integration, stability and detection accuracy, especially under the influence of external deformation and environmental factors, which affect the accuracy and reliability of detection results.
By tightly combining the silk fiber membrane with a layer of silver nanoparticles and gold seeds to enhance the conductivity and stability of the fiber, silk fabric sensors are used to provide reliable detection results in muscle stress strain and human biomolecule detection.
It achieves high stability in changing environments and reliable performance in long-term use, ensuring the consistency and sensitivity of detection results, making it suitable for wearable device applications.
Smart Images

Figure CN118857518A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of flexible sensors and relates to a silk fabric sensor. The present invention also relates to a method for preparing the silk fabric sensor and the application of the silk fabric sensor in muscle stress and strain detection and human biological molecule detection. Background Art
[0002] In modern biomedical research and clinical diagnosis, the detection of biomechanical properties and biochemical composition is crucial. Existing biomechanical sensors and biomolecular sensors have deficiencies in sensitivity, stability and versatility. Existing biomechanical sensors mostly use principles such as piezoresistance, piezoelectricity and capacitance, and are often made of hard materials. Their sensitivity and response speed need to be improved, and they are not suitable for flexible and wearable applications. Biomolecular sensors rely on optical, electrochemical or fluorescence technology. Although they are highly sensitive, they are expensive, complex to operate, and difficult to monitor in real time. Flexible sensors still face challenges in multifunctional integration, stability and detection accuracy, and are easily affected by external deformation and environmental factors.
[0003] In recent years, flexible sensors have gradually gained attention in wearable devices due to their good flexibility and biocompatibility. However, existing flexible sensors still face many challenges in terms of multifunctional integration, stability and detection accuracy. For example, the electrical properties of many flexible sensors will change significantly when subjected to external deformation, affecting the accuracy of the detection results. In addition, flexible sensors are easily affected by environmental factors (such as humidity, temperature, etc.) during long-term use, resulting in performance degradation. Amyotrophic lateral sclerosis (ALS) is a progressive neurodegenerative disease accompanied by significant changes in biomechanical and biochemical signals. Traditional detection methods such as electroencephalogram (EEG) and electromyography (EMG), although they can provide certain information, are complex to operate and have poor patient experience, making it difficult to achieve long-term, real-time monitoring. Summary of the invention
[0004] The purpose of the present invention is to provide a silk fabric sensor. The silk fiber membrane of the silk fabric sensor is tightly combined with the gold seed layer through silver nanoparticles, which enhances the conductivity and stability of the fiber, provides a solution for the reliability of flexible sensors in a changing environment, and solves the problem in the prior art that the electrical properties of flexible sensors will change significantly when subjected to external deformation, thereby affecting the accuracy of the detection results.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned silk fabric sensor.
[0006] The third object of the present invention is to provide an application of a silk fabric sensor in muscle stress and strain detection and human biomolecule detection.
[0007] The technical solution adopted by the present invention is a silk fabric sensor, comprising an interpolation electrode placed on a flexible substrate, the interpolation electrode is covered with a silk fiber membrane, a sealing ring is arranged above the silk fiber membrane at the edge of the silk fiber membrane, and a packaging layer is arranged above the sealing ring.
[0008] The second technical solution adopted by the present invention is: a method for preparing a silk fabric sensor, and preparing the silk fabric sensor is specifically as follows:
[0009] Step 1, preparing a silk fiber membrane;
[0010] Step 2: Place an interpolation electrode on the flexible substrate, then cover the interpolation electrode with the prepared silk fiber membrane, and ensure that the silk fiber membrane is in full contact with the interpolation electrode, then place a sealing ring on the edge of the silk fiber membrane, and finally encapsulate the whole above the sealing ring to form an encapsulation layer.
[0011] The second technical solution of the present invention is also characterized in that:
[0012] Step 1 is as follows:
[0013] Step 1.1, pre-treating silk fibers;
[0014] Step 1.2, depositing a gold seed layer on the surface of the pretreated silk fiber;
[0015] Step 1.3, in situ growth of silver ions is performed on the gold seed layer, so that the silver ions grow on the gold seed layer to form silver nanoparticles and form a silk fiber membrane.
[0016] Step 1.1 is specifically as follows: after taking out the natural silk fiber, soak it in acetone for 20-30 minutes, and then wash it thoroughly with deionized water until the washing liquid is clear; then soak the washed silk fiber in alcohol for 20-30 minutes, and then wash the silk fiber again with deionized water until the washing liquid is clear, and then dry it naturally at room temperature.
[0017] Step 1.2 is as follows:
[0018] Step 1.2.1, HAuCl 4 Dissolve the chloroauric acid solution in deionized water to prepare a concentration of 10-20 mM, then immerse the silk fiber in the chloroauric acid solution and let it stand at room temperature to allow the chloroauric acid to be evenly adsorbed on the surface of the silk fiber;
[0019] Step 1.2.2, adding a reducing agent sodium borohydride solution dropwise to the chloroauric acid solution of step 1.2.1, and stirring for 1-3 minutes to allow gold nanoparticles to deposit on the surface of the silk fiber to form a gold seed layer;
[0020] Step 1.2.3, taking out the silk fibers after the reaction in step 1.2.2, washing them with deionized water for several times until the washing liquid is clear and colorless, and then drying them at room temperature;
[0021] Step 1.2.4, take out the dried silk fiber and repeat the steps 1.2.1-1.2.3 at least 3 times to obtain silk fiber with a gold seed layer deposited.
[0022] In step 1.2.2, the concentration of the sodium borohydride solution is 0.5-1 M, and the volume ratio of the chloroauric acid solution to the sodium borohydride solution is 1.5:1.
[0023] Step 1.3 is as follows:
[0024] Step 1.3.1, prepare a 10-20 mM silver nitrate solution and a 0.1 M ascorbic acid solution;
[0025] Step 1.3.2, adding 5wt% PVP solution, acetonitrile, anhydrous ethanol, the silver nitrate solution and ascorbic acid solution prepared in step 1.3.1 to deionized water, and stirring to form a growth solution, wherein the volume ratio of the PVP solution, acetonitrile, anhydrous ethanol, silver nitrate solution, ascorbic acid solution and deionized water is 20:20:20:1.5:1:20;
[0026] Step 1.3.3, placing the silk fibers treated in step 1.2 in a growth solution and subjecting them to magnetic stirring at -5 to -10°C for 10 to 30 minutes, so that the silver ions grow on the gold seed layer to form silver nanoparticles;
[0027] Step 1.3.4, taking out the silk fibers after the reaction in step 1.3.3, washing them several times with deionized water until the washing liquid is clear, and then drying them at room temperature;
[0028] Step 1.3.5, placing the dried silk fibers in a growth solution and repeating the process of steps 1.3.3-1.3.4 at least three times to obtain a silk fiber membrane.
[0029] The third technical solution adopted by the present invention is the application of silk fabric sensors in muscle stress and strain detection and human biological molecule detection. The silk fabric sensors prepared by the above method are used for muscle stress and strain detection and human biological molecule detection.
[0030] When conducting muscle stress and strain testing, the silk fabric sensor is attached to the location of the muscle to be tested and fixed with medical tape. The interpolation electrode of the silk fabric sensor is connected to the electrochemical workstation to detect changes in biological stress and strain by monitoring different muscle movements.
[0031] When conducting human biomolecule detection, the silk fiber membrane in the silk fabric sensor is placed in a solution containing specific biomolecules and then monitored using a handheld Raman spectrometer to identify the biomolecules therein.
[0032] The beneficial effects of the present invention are:
[0033] The preparation method of the silk fabric sensor of the present invention comprises the following steps: immersing the silk fiber in a chloroauric acid (HAuCl4) solution, the chloroauric acid is uniformly adsorbed on the fiber surface, a sodium borohydride (NaBH4) solution is added dropwise, the chloroauric acid is reduced to gold nanoparticles, a gold seed layer is formed, the silk fiber of the gold seed layer is placed in a silver nitrate (AgNO3) solution, and an ascorbic acid solution is added dropwise, the ascorbic acid is used as a reducing agent, the silver ions in the silver nitrate are reduced to silver nanoparticles, the silver nanoparticles are uniformly grown on the gold seed surface, and the ascorbic acid is stirred in a glass bottle, so that the silver nitrate is reduced by ascorbic acid to form silver nanoparticles; the silver particles are uniformly grown on the gold seed layer, the flexible silk fiber and the silver nanoparticles are ensured to have excellent flexibility and biocompatibility, and are very suitable for use in wearable devices. The present invention enhances the conductivity and stability of the fiber by tightly combining the silver nanoparticles with the gold seed layer, and ensures the reliable performance of the sensor in a changing environment. This result proves the excellent durability and long-term reliability of the sensor, and provides an important material basis for the development of silk fiber-based piezoresistive sensors.
[0034] The silk fabric sensor prepared by using the silk fiber of the present invention can still maintain high stability during long-term use, thereby ensuring the reliability and consistency of the detection results.
[0035] The application of the silk fabric sensor of the present invention in biological stress detection and biological molecule detection provides scientific support for health monitoring and disease diagnosis. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a principle flow chart of the method for preparing the silk fiber membrane in the method for preparing the silk fabric sensor of the present invention;
[0037] Figure 2 is a scanning electron microscope image of the original silk fiber used in the embodiment of the method for preparing the silk fabric sensor of the present invention;
[0038] Figure 3 is a scanning electron microscope (SEM) image of the silk fiber prepared in Example 1 of the present invention;
[0039] Figure 4 is a scanning electron microscope (SEM) image of a cross section of a silk fiber prepared in Example 1 of the present invention;
[0040] Figure 5is an infrared spectrum of the silk fiber prepared in Example 1 of the present invention;
[0041] Figure 6 is an energy dispersive spectroscopy (EDS) graph of the silk fiber prepared in Example 1 of the present invention;
[0042] Figure 7 This is a graph showing the conductivity of the silk fiber prepared in Example 1 of the present invention tested at different times in a silk fabric sensor;
[0043] Figure 8 is a schematic diagram of the structure of the silk fabric sensor after assembly according to Example 6 of the present invention;
[0044] Fig. 9 is a physical picture of the assembled silk fabric sensor of Example 6 of the present invention;
[0045] Fig.10a is an example diagram of the application of the assembled silk fabric sensor in biological stress detection in deltoid muscle according to Example 7 of the present invention;
[0046] Fig.10b is an example diagram of the application of the assembled silk fabric sensor in biological stress detection on the biceps brachii in Example 7 of the present invention;
[0047] Fig.10c This is an example diagram of the assembled silk fabric sensor of Example 7 of the present invention being applied to the radial wrist flexor flexor arm in biological stress detection;
[0048] Fig.11 is a flowchart of the support vector machine (SVM) used in Example 9 of the present invention;
[0049] Fig.12 is a schematic diagram of monitoring using a handheld Raman spectrometer in Example 8 of the present invention;
[0050] Fig.13 is a biomolecule detection diagram of the thiuram solution monitored in Example 8 of the present invention;
[0051] Fig.14 It is a 40-line waterfall diagram of the thiuram molecule in Example 8 of the present invention;
[0052] Fig.15 is a Raman spectrum of human sweat obtained in Example 8 of the present invention;
[0053] Fig.16 is a cycle test diagram of the silk fabric sensor according to Example 6 of the present invention;
[0054] Fig.17 is a response time diagram of the silk fabric sensor according to Example 6 of the present invention;
[0055] Fig.18 is a sensitivity diagram of the silk fabric sensor according to Example 6 of the present invention;
[0056] Fig.19 3 and 4 are different frequency response diagrams of the silk fabric sensor according to Example 6 of the present invention.
[0057] In the figure: 1. Flexible substrate, 2. Interpolation electrode, 3. Silk fiber membrane, 4. Sealing ring, 5. Packaging layer. DETAILED DESCRIPTION
[0058] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0059] The preparation method of the silk fabric sensor of the present invention is specifically as follows:
[0060] Step 1, preparing the silk fiber membrane 3, specifically:
[0061] Step 1.1, pre-treating the silk fiber, specifically: taking out the natural silk fiber and soaking it in acetone for 20-30 minutes, then washing it thoroughly with deionized water until the washing liquid is clear; then soaking the washed silk fiber in alcohol for 20-30 minutes, then washing it thoroughly with deionized water again until the washing liquid is clear, and then drying it naturally at room temperature;
[0062] Step 1.2, depositing a gold seed layer on the surface of the pretreated silk fiber, specifically:
[0063] Step 1.2.1, HAuCl 4 Dissolve the chloroauric acid solution in deionized water to prepare a concentration of 10-20 mM, then immerse the silk fiber in the chloroauric acid solution and let it stand at room temperature to allow the chloroauric acid to be evenly adsorbed on the surface of the silk fiber;
[0064] Step 1.2.2: Add the reducing agent sodium borohydride (NaBH) dropwise to the chloroauric acid solution in step 1.2.1. 4 solution, and keep stirring for 1-3 minutes to allow gold nanoparticles to deposit on the surface of the silk fibers to form a gold seed layer, wherein the concentration of the sodium borohydride solution is 0.5-1M, and the volume ratio of the chloroauric acid solution to the sodium borohydride solution is 1.5:1;
[0065] Step 1.2.3, taking out the silk fibers after the reaction in step 1.2.2, washing them with deionized water for several times until the washing liquid is clear and colorless, and then drying them at room temperature;
[0066] Step 1.2.4, taking out the dried silk fiber and repeating the steps 1.2.1-1.2.3 at least 3 times to obtain the silk fiber deposited to form a gold seed layer;
[0067] Step 1.3, in situ growth of silver ions on the gold seed layer, so that the silver ions grow on the gold seed layer to form silver nanoparticles and form a silk fiber membrane. Step 1.3.1, prepare silver nitrate AgNO with a concentration of 10-20mM 3 solution and ascorbic acid solution with a concentration of 0.1 M;
[0068] Step 1.3.2, adding 5wt% PVP solution, acetonitrile, anhydrous ethanol, the silver nitrate solution and ascorbic acid solution prepared in step 1.3.1 to deionized water, and stirring to form a growth solution, wherein the volume ratio of the PVP solution, acetonitrile, anhydrous ethanol, silver nitrate solution, ascorbic acid solution and deionized water is 20:20:20:1.5:1:20;
[0069] Step 1.3.3, placing the silk fibers treated in step 1.2 in a growth solution and subjecting them to magnetic stirring at -5 to -10°C for 10 to 30 minutes, so that the silver ions grow on the gold seed layer to form silver nanoparticles;
[0070] Step 1.3.4, taking out the silk fibers after the reaction in step 1.3.3, washing them several times with deionized water until the washing liquid is clear, and then drying them at room temperature;
[0071] Step 1.3.5, placing the dried silk fiber in a growth solution and repeating the process of steps 1.3.3-1.3.4 at least three times to obtain a silk fiber membrane;
[0072] Step 2, placing the interpolation electrode 2 on the flexible substrate 1, and then covering the interpolation electrode 2 with the prepared silk fiber membrane 3, and ensuring that the silk fiber membrane 3 is in full contact with the interpolation electrode 2, and then placing a sealing ring 4 above the silk fiber membrane 3 at its edge, and finally encapsulating the whole above the sealing ring 4 to form an encapsulation layer 5.
[0073] The principle of the present invention is as follows Figure 1As shown in the figure, silk fibers are rich in amino (—NH2), carboxyl (—COOH), amide (—CONH2) and hydroxyl (—OH) functional groups, which can coordinate and bond with the surface electrons of gold nanoparticles to form a composite material with high stability; on the basis of gold nanoparticles, silver nanoparticles are uniformly grown through chemical coupling, and this process benefits from the electrostatic attraction and coordination bond between gold and silver nanoparticles. Specifically, gold nanoparticles are negatively charged, while silver ions in the silver precursor solution are positively charged. When the two are in contact, the positively charged silver ions are attracted by the negatively charged gold nanoparticles and form a stable bond on their surface. In addition, the coordination reaction between silver atoms and the surface electrons of gold nanoparticles further strengthens this bond, giving the material excellent chemical and thermal stability, allowing it to maintain its performance unchanged in a changing environment. This feature contributes to the uniform distribution of silver nanoparticles on silk fibers, providing an important material basis for the development of piezoresistive sensors based on silk fibers. The uniform deposition of silver nanoparticles on silk fibers was achieved through the following chemical reaction steps: by immersing silk fibers in chloroauric acid (HAuCl4) solution, chloroauric acid was uniformly adsorbed on the fiber surface, sodium borohydride (NaBH4) solution was added dropwise, chloroauric acid was reduced to gold nanoparticles, and a gold seed layer was formed. The silk fibers with the gold seed layer were placed in a silver nitrate (AgNO3) solution, and ascorbic acid solution was added dropwise. Ascorbic acid was used as a reducing agent to reduce the silver ions in the silver nitrate to silver nanoparticles, which grew uniformly on the gold seed surface. The mixture was stirred in a glass bottle, so that the silver nitrate was reduced by ascorbic acid to form silver nanoparticles, and the silver particles grew uniformly on the gold seed layer. Through this chemical reaction process, the silver nanoparticles were tightly combined with the gold seed layer, which enhanced the conductivity and stability of the fiber and ensured the reliable performance of the sensor in a changing environment. This method not only improved the chemical and thermal stability of the material, but also provided an important material basis for the development of silk fiber-based piezoresistive sensors.
[0074] Examples 1-5 are different implementation cases of preparing the silk fiber membrane in step 1, as follows:
[0075] Example 1
[0076] The method for preparing silk fiber membrane, the scanning electron microscope image of the original silk fiber used is as follows Figure 2 As shown, the specific steps are as follows:
[0077] Step 1.1, taking out the natural silk fiber and soaking it in acetone for 30 minutes, then washing it thoroughly with deionized water until the washing solution is clear; then soaking the washed silk fiber in alcohol for 30 minutes, then washing it thoroughly with deionized water again until the washing solution is clear, and then drying it naturally at room temperature;
[0078] Step 1.2, depositing a gold seed layer on the surface of the pretreated silk fiber, specifically:
[0079] Step 1.2.1, HAuCl 4 Dissolve chloroauric acid solution in deionized water to prepare a 10 mM concentration, then immerse the silk fiber in the chloroauric acid solution and let it stand at room temperature to allow the chloroauric acid to be evenly adsorbed on the surface of the silk fiber;
[0080] Step 1.2.2, take out the silk fiber in step 1.2.1 from 3 ml of chloroauric acid solution, add dropwise into 4.5 ml of 0.6 M sodium borohydride (NaBH4) solution, and then take out the silk fiber;
[0081] Step 1.2.3, taking out the silk fibers after the reaction in step 1.2.2, washing them with deionized water for several times until the washing liquid is clear and colorless, and then drying them at room temperature;
[0082] Step 1.2.4, taking out the dried silk fiber and repeating the steps 1.2.1-1.2.3 for 6 times to obtain the silk fiber deposited to form a gold seed layer;
[0083] Step 1.3, in situ growth of silver ions on the gold seed layer, so that the silver ions grow on the gold seed layer to form silver nanoparticles and form a silk fiber membrane, specifically:
[0084] Step 1.3.1, prepare silver nitrate (AgNO) at a concentration of 10 mM 3 ) solution and a 0.1 M ascorbic acid solution;
[0085] Step 1.3.2, adding 5wt% PVP solution, acetonitrile, anhydrous ethanol, the silver nitrate solution and ascorbic acid solution prepared in step 1.3.1 to deionized water, and stirring to form a growth solution, wherein the volumes of the PVP solution, acetonitrile, anhydrous ethanol, silver nitrate solution, ascorbic acid solution and deionized water are 2000ml, 2000ml, 2000ml, 150ml, 100ml and 2000ml respectively;
[0086] Step 1.3.3, placing the silk fiber treated in step 1.2 in a growth solution and subjecting it to magnetic stirring for 20 minutes at -8°C, so that the silver ions grow on the gold seed layer to form silver nanoparticles; Step 1.3.4, taking out the silk fiber after the reaction in step 1.3.3, washing it several times with deionized water until the washing solution is clear, and then drying it at room temperature;
[0087] Step 1.3.5, placing the dried silk fiber in the growth solution and repeating the process of steps 1.3.3-1.3.4 for 6 times to obtain a silk fiber membrane. The silk fiber is as follows: Figure 3 As shown, the conductive network structure formed by the growth of silver nanoparticles on silk fibers.
[0088] like Figure 4 The figure shows a scanning electron microscope image of a cross section of a silk fiber after the gold seeds and silver particles are grown in situ in this embodiment. Figure 4 It can be seen that the surface of the treated silk fiber is evenly covered with silver particles, which are clearly visible in the cross-sectional image. The silver particles are evenly distributed throughout the fiber surface and inside, indicating that the treatment is effective.
[0089] like Figure 5 The figure shows the FT-IR spectrum of the silk fiber and the gold nanoparticles after the interaction in this embodiment; the FT-IR spectrum further confirms the chemical interaction between the silk fiber and the gold nanoparticles. -1 、1665cm -1 、1229cm -1 and 639cm -1 The absorption peaks at correspond to the stretching vibrations of -NH-, -C=O-, and -CN- functional groups in the silk fibers and the bending vibration of the -C=O- functional group. These typical absorption peaks indicate that the gold nanoparticles are uniformly fixed on the surface of the silk fibers by interacting with these active functional groups on the silk fibers.
[0090] like Figure 6 As shown in the figure, it is an energy dispersive X-ray spectrum (EDS) diagram of the surface of the silk fiber prepared in this embodiment. The results of the energy spectrum (EDS) analysis show that the surface of the silk fiber is rich in carbon (C), nitrogen (N), oxygen (O), gold (Au) and silver (Ag) elements; the presence of these elements is directly related to the chemical coupling between the silk fiber and the gold and silver nanoparticles. In particular, the detection of Au and Ag confirms that the gold and silver nanoparticles have been evenly covered on the silk fiber. Through EDS element mapping, the uniform distribution of C, O, Au and Ag atoms on the surface of the silk fiber is observed, which further proves the stable combination between the gold and silver nanoparticles and the silk fiber.
[0091] like Figure 7As shown in the figure, the conductivity test diagram of the silk fiber after multiple adsorption of silver nanoparticles in this embodiment is carried out. The test results show that the conductivity of the silk fiber reaches the best when the silver nanoparticles are adsorbed 6 times after 9 gold seed depositions. However, when the silver nanoparticles are adsorbed more times, the conductivity decreases instead. This phenomenon may be caused by the uneven adsorption and agglomeration of silver nanoparticles on the fiber surface. Too many silver nanoparticles gather on the surface, causing the silver particles between the fibers to break contact, destroying the continuous conductive path, thereby affecting the overall conductivity of the sensor.
[0092] Example 2
[0093] The method for preparing silk fiber membrane, the scanning electron microscope image of the original silk fiber used is as follows Figure 2 As shown, the specific steps are as follows:
[0094] Step 1.1, taking out the natural silk fiber and soaking it in acetone for 30 minutes, then washing it thoroughly with deionized water until the washing solution is clear; then soaking the washed silk fiber in alcohol for 30 minutes, then washing it thoroughly with deionized water again until the washing solution is clear, and then drying it naturally at room temperature;
[0095] Step 1.2, depositing a gold seed layer on the surface of the pretreated silk fiber, specifically:
[0096] Step 1.2.1, HAuCl 4 Dissolve chloroauric acid solution in deionized water to prepare a 12.5 mM concentration, then immerse the silk fiber in the chloroauric acid solution and allow it to stand at room temperature to allow the chloroauric acid to be evenly adsorbed on the surface of the silk fiber;
[0097] Step 1.2.2, take out the silk fiber in step 1.2.1 from 3 ml of chloroauric acid solution, add dropwise into 4.5 ml of 0.7 M sodium borohydride (NaBH4) solution, and then take out the silk fiber;
[0098] Step 1.2.3, taking out the silk fibers after the reaction in step 1.2.2, washing them with deionized water for several times until the washing liquid is clear and colorless, and then drying them at room temperature;
[0099] Step 1.2.4, taking out the dried silk fiber and repeating the steps 1.2.1-1.2.3 for 9 times to obtain the silk fiber deposited to form a gold seed layer;
[0100] Step 1.3, in situ growth of silver ions on the gold seed layer, so that the silver ions grow on the gold seed layer to form silver nanoparticles and form a silk fiber membrane, specifically:
[0101] Step 1.3.1, prepare silver nitrate (AgNO) at a concentration of 12.5 mM 3 ) solution and a 0.1 M ascorbic acid solution;
[0102] Step 1.3.2, adding 5wt% PVP solution, acetonitrile, anhydrous ethanol, the silver nitrate solution and ascorbic acid solution prepared in step 1.3.1 to deionized water, and stirring to form a growth solution, wherein the volumes of the PVP solution, acetonitrile, anhydrous ethanol, silver nitrate solution, ascorbic acid solution and deionized water are 2000ml, 2000ml, 2000ml, 150ml, 100ml and 2000ml respectively;
[0103] Step 1.3.3, placing the silk fibers treated in step 1.2 in a growth solution and subjecting them to magnetic stirring for 20 minutes at -8°C, so that the silver ions grow on the gold seed layer to form silver nanoparticles;
[0104] Step 1.3.4, taking out the silk fibers after the reaction in step 1.3.3, washing them several times with deionized water until the washing liquid is clear, and then drying them at room temperature;
[0105] Step 1.3.5, placing the dried silk fibers in a growth solution and repeating the process of steps 1.3.3-1.3.4 for 9 times to obtain a silk fiber membrane.
[0106] Example 3
[0107] The method for preparing silk fiber membrane, the scanning electron microscope image of the original silk fiber used is as follows Figure 2 As shown, the specific steps are as follows:
[0108] Step 1.1, taking out the natural silk fiber and soaking it in acetone for 30 minutes, then washing it thoroughly with deionized water until the washing solution is clear; then soaking the washed silk fiber in alcohol for 30 minutes, then washing it thoroughly with deionized water again until the washing solution is clear, and then drying it naturally at room temperature;
[0109] Step 1.2, depositing a gold seed layer on the surface of the pretreated silk fiber, specifically:
[0110] Step 1.2.1, HAuCl 4 Dissolve chloroauric acid solution in deionized water to prepare a 15 mM concentration, then immerse the silk fiber in the chloroauric acid solution and allow it to stand at room temperature to allow the chloroauric acid to be evenly adsorbed on the surface of the silk fiber;
[0111] Step 1.2.2, take out the silk fiber in step 1.2.1 from 3 ml of chloroauric acid solution, add dropwise into 4.5 ml of 0.8 M sodium borohydride (NaBH4) solution, and then take out the silk fiber;
[0112] Step 1.2.3, taking out the silk fibers after the reaction in step 1.2.2, washing them with deionized water for several times until the washing liquid is clear and colorless, and then drying them at room temperature;
[0113] Step 1.2.4, taking out the dried silk fiber and repeating the steps 1.2.1-1.2.3 for 9 times to obtain the silk fiber deposited to form a gold seed layer;
[0114] Step 1.3, in situ growth of silver ions on the gold seed layer, so that the silver ions grow on the gold seed layer to form silver nanoparticles and form a silk fiber membrane, specifically:
[0115] Step 1.3.1, prepare silver nitrate (AgNO) at a concentration of 15 mM 3 ) solution and a 0.1 M ascorbic acid solution;
[0116] Step 1.3.2, adding 5wt% PVP solution, acetonitrile, anhydrous ethanol, the silver nitrate solution and ascorbic acid solution prepared in step 1.3.1 to deionized water, and stirring to form a growth solution, wherein the volumes of the PVP solution, acetonitrile, anhydrous ethanol, silver nitrate solution, ascorbic acid solution and deionized water are 2000ml, 2000ml, 2000ml, 150ml, 100ml and 2000ml respectively;
[0117] Step 1.3.3, placing the silk fiber treated in step 1.2 in a growth solution and subjecting it to magnetic stirring for 20 minutes at -8°C, so that the silver ions grow on the gold seed layer to form silver nanoparticles; Step 1.3.4, taking out the silk fiber after the reaction in step 1.3.3, washing it several times with deionized water until the washing solution is clear, and then drying it at room temperature;
[0118] Step 1.3.5, place the dried silk fibers in a growth solution and repeat the process of steps 1.3.3-1.3.4 three times to obtain a silk fiber membrane.
[0119] Example 4
[0120] The method for preparing silk fiber membrane, the scanning electron microscope image of the original silk fiber used is as follows Figure 2 As shown, the specific steps are as follows:
[0121] Step 1.1, taking out the natural silk fiber and soaking it in acetone for 30 minutes, then washing it thoroughly with deionized water until the washing solution is clear; then soaking the washed silk fiber in alcohol for 30 minutes, then washing it thoroughly with deionized water again until the washing solution is clear, and then drying it naturally at room temperature;
[0122] Step 1.2, depositing a gold seed layer on the surface of the pretreated silk fiber, specifically:
[0123] Step 1.2.1, HAuCl 4 Dissolve chloroauric acid solution in deionized water to prepare a 17.5 mM concentration, then immerse the silk fiber in the chloroauric acid solution and allow it to stand at room temperature to allow the chloroauric acid to be evenly adsorbed on the surface of the silk fiber;
[0124] Step 1.2.2, take out the silk fiber in step 1.2.1 from 3 ml of chloroauric acid solution, add dropwise into 4.5 ml of 0.9 M sodium borohydride (NaBH4) solution, and then take out the silk fiber;
[0125] Step 1.2.3, taking out the silk fibers after the reaction in step 1.2.2, washing them with deionized water for several times until the washing liquid is clear and colorless, and then drying them at room temperature;
[0126] Step 1.2.4, taking out the dried silk fiber and repeating the steps 1.2.1-1.2.3 for 9 times to obtain the silk fiber deposited to form a gold seed layer;
[0127] Step 1.3, in situ growth of silver ions on the gold seed layer, so that the silver ions grow on the gold seed layer to form silver nanoparticles and form a silk fiber membrane, specifically:
[0128] Step 1.3.1, prepare silver nitrate (AgNO) at a concentration of 17.5 mM 3 ) solution and 0.1M ascorbic acid (C6H8O6) solution;
[0129] Step 1.3.2, adding 5wt% PVP solution, acetonitrile, anhydrous ethanol, the silver nitrate solution and ascorbic acid solution prepared in step 1.3.1 to deionized water, and stirring to form a growth solution, wherein the volumes of the PVP solution, acetonitrile, anhydrous ethanol, silver nitrate solution, ascorbic acid solution and deionized water are 2000ml, 2000ml, 2000ml, 150ml, 100ml and 2000ml respectively;
[0130] Step 1.3.3, placing the silk fibers treated in step 1.2 in a growth solution and subjecting them to magnetic stirring for 20 minutes at -8°C, so that the silver ions grow on the gold seed layer to form silver nanoparticles;
[0131] Step 1.3.4, taking out the silk fibers after the reaction in step 1.3.3, washing them several times with deionized water until the washing liquid is clear, and then drying them at room temperature;
[0132] Step 1.3.5, placing the dried silk fibers in a growth solution and repeating the process of steps 1.3.3-1.3.4 for 6 times to obtain a silk fiber membrane.
[0133] Example 5
[0134] The method for preparing silk fiber membrane, the scanning electron microscope image of the original silk fiber used is as follows Figure 2 As shown, the specific steps are as follows:
[0135] Step 1.1, taking out the natural silk fiber and soaking it in acetone for 30 minutes, then washing it thoroughly with deionized water until the washing solution is clear; then soaking the washed silk fiber in alcohol for 30 minutes, then washing it thoroughly with deionized water again until the washing solution is clear, and then drying it naturally at room temperature;
[0136] Step 1.2, depositing a gold seed layer on the surface of the pretreated silk fiber, specifically:
[0137] Step 1.2.1, HAuCl 4 Dissolve 20 mM chloroauric acid solution in deionized water, then immerse the silk fiber in the chloroauric acid solution and let it stand at room temperature to allow the chloroauric acid to be evenly adsorbed on the surface of the silk fiber;
[0138] Step 1.2.2, take out the silk fiber in step 1.2.1 from 3 ml of chloroauric acid solution, add dropwise into 4.5 ml of 1 M sodium borohydride (NaBH4) solution, and then take out the silk fiber;
[0139] Step 1.2.3, taking out the silk fibers after the reaction in step 1.2.2, washing them with deionized water for several times until the washing liquid is clear and colorless, and then drying them at room temperature;
[0140] Step 1.2.4, taking out the dried silk fiber and repeating the steps 1.2.1-1.2.3 for 9 times to obtain the silk fiber deposited to form a gold seed layer;
[0141] Step 1.3, in situ growth of silver ions on the gold seed layer, so that the silver ions grow on the gold seed layer to form silver nanoparticles and form a silk fiber membrane, specifically:
[0142] Step 1.3.1, prepare silver nitrate (AgNO) at a concentration of 20 mM 3 ) solution and 0.1M ascorbic acid (C6H8O6) solution;
[0143] Step 1.3.2, adding 5wt% PVP solution, acetonitrile, anhydrous ethanol, the silver nitrate solution and ascorbic acid solution prepared in step 1.3.1 to deionized water, and stirring to form a growth solution, wherein the volumes of the PVP solution, acetonitrile, anhydrous ethanol, silver nitrate solution, ascorbic acid solution and deionized water are 2000ml, 2000ml, 2000ml, 150ml, 100ml and 2000ml respectively;
[0144] Step 1.3.3, placing the silk fibers treated in step 1.2 in a growth solution and subjecting them to magnetic stirring for 20 minutes at -8°C, so that the silver ions grow on the gold seed layer to form silver nanoparticles;
[0145] Step 1.3.4, taking out the silk fibers after the reaction in step 1.3.3, washing them several times with deionized water until the washing liquid is clear, and then drying them at room temperature;
[0146] Step 1.3.5, placing the dried silk fibers in a growth solution and repeating the process of steps 1.3.3-1.3.4 for 9 times to obtain a silk fiber membrane.
[0147] Example 6
[0148] The silk fabric sensor is prepared by using the silk fiber membrane of Example 1, and its structure is as follows Figure 8 As shown, an interpolation electrode 2 is placed on a flexible substrate 1, a silk fiber membrane 3 is covered on the interpolation electrode 2, a sealing ring 4 is arranged above the silk fiber membrane 3 at the edge of the silk fiber membrane 3, and a packaging layer 5 is arranged above the sealing ring 4, as shown in FIG. Fig. 9 The figure shows a real picture of the silk fabric sensor actually manufactured in this embodiment.
[0149] A method for preparing a silk fabric sensor, preparing a silk fabric sensor, specifically according to the following steps: using Example 3 to prepare a silk fiber membrane 3, then placing an interpolation electrode 2 on a flexible substrate 1, then covering the interpolation electrode 2 with the silk fiber membrane 3 prepared in step 1, and ensuring that the silk fiber membrane 3 is in full contact with the interpolation electrode 2, then placing a sealing ring 4 above the silk fiber membrane 3 at its edge, and finally encapsulating the whole above the sealing ring 4 to form an encapsulation layer 5, covering the encapsulation layer to protect the internal structure of the sensor and provide additional mechanical strength.
[0150] The flexible substrate 1 used in this embodiment is a PMMA flexible substrate.
[0151] In order to verify the performance of the present invention, the silk fabric sensor of this embodiment was subjected to 5000 cycles of testing under a pressure of 5 kPa. The results showed that the current response of the silk fabric sensor remained highly consistent with almost no obvious attenuation. Fig.16 As shown, it can be proved that the silk fabric sensor prepared by using the silk fiber of the present invention can still maintain high stability during long-term use, ensuring the reliability and consistency of the detection results.
[0152] like Fig.17 As shown, the current response time of the silk fabric sensor made in this embodiment, the figure shows the delay time of the current response during the pressure release process, which is about 153 milliseconds and 68 milliseconds respectively, which proves that the sensor has a fast response speed and recovery ability.
[0153] like Fig.18 As shown in the figure, the sensitivity of the silk fabric sensor made in this embodiment is as follows. It can be seen from the figure that the sensor is 2 =0.96) and high pressure (R 2 =0.98) range, and the pressure sensitivity was 16.82±1.50KPa. -1 and 161.34±13.19KPa -1 , which indicates that the sensor has high sensitivity and good linearity in a wide pressure range.
[0154] like Fig.19 As shown, the responses of the silk fabric sensor produced in this embodiment at different frequencies are shown, which demonstrates the current responses of the sensor at different frequencies (0.2Hz, 0.4Hz, 0.6Hz, 0.8Hz, 1Hz). It can be seen that the current responses of the sensor at different frequencies remain highly consistent without obvious attenuation, which proves the high stability and reliability of the sensor in long-term use.
[0155] Example 7
[0156] On the basis of Example 6, the application of the silk fabric sensor of the present invention in muscle stress and strain detection and human biomolecule detection, using the silk fabric sensor to perform muscle stress and strain detection and human biomolecule detection;
[0157] When conducting biological stress detection, the silk fabric sensor is attached to the position of the muscle to be detected and fixed with medical tape. The interpolation electrode 2 of the silk fabric sensor is connected to the electrochemical workstation to detect changes in biological stress by monitoring different muscle movements.
[0158] like Figure 10a-Figure 10c, which is an example diagram of the application of the silk fabric sensor assembled in Example 6 in biological stress detection; by attaching the silk fabric sensor to the skin surface at the position of the muscle to be detected, the biological stress signal can be monitored in real time. In practical applications, the sensor can sensitively capture the tiny deformation of the skin surface caused by different biological stresses (such as heartbeat, breathing, muscle contraction, etc.) and convert it into an electrical signal output. The test results show that the sensor exhibits high sensitivity and stability under different biological stresses. Fig.10a The sensor's current signal changes when the deltoid muscle is doing arm-raising exercise. It can be seen that the sensor's current response changes significantly during the arm-raising process, proving its high sensitivity to muscle movement; Fig.10b The sensor's current signal changes when the biceps brachii is in normal and flexed state are shown. It can be seen that the sensor's current response changes significantly during normal and flexed state, proving its high sensitivity to muscle movement. Fig.10c The sensor's current signal changes when the radial wrist flexor muscle is bent are shown. The results show that the sensor's current response remains consistent and stable under different muscle states, proving its excellent durability and reliability. It can be seen that the sensor of the present invention can accurately record these biological stress signals, reflecting its high sensitivity and high stability. This biological stress detection capability gives the sensor broad application prospects in the fields of medical care, sports monitoring, etc.
[0159] Example 8
[0160] On the basis of Example 6, the application of the silk fabric sensor of the present invention is to place the silk fiber membrane 3 prepared in Example 1 in a solution containing specific biomolecules during biomolecule detection, and then monitor it using a handheld Raman spectrometer. The monitoring diagram is as follows: Fig.12 As shown, to identify the biomolecules therein.
[0161] In this embodiment, the prepared silk fiber membrane 3 is placed in thiuram solutions with different concentrations to obtain Raman spectra of the standard biological molecule thiuram at different concentrations, as shown in FIG. Fig. 9 As shown;
[0162] like Fig.13 As shown, the biomolecule detection diagram of the thiuram solution monitored in this embodiment shows the actual detection results of the sensor in biomolecule detection.
[0163] like Fig.14As shown, there are 40 waterfall graphs of the thiuram molecule used in this embodiment. The Raman spectra of the thiuram molecule at different concentrations are displayed in three dimensions in the form of waterfall graphs, which enhances the visualization of the data, helps to more intuitively understand and analyze the spectral characteristics of the thiuram molecule, and provides an important reference for the research and application of biomolecule detection. The result of the relative standard deviation (RSD) of 13.75% further verifies the stability and accuracy of the data.
[0164] The silk fiber membrane 3 prepared in Example 1 was placed in human sweat to obtain a Raman spectrum of human sweat, as shown in FIG. Fig.15 As shown in the figure, the Raman spectrum of human sweat reveals the molecular structure information of various components in sweat in detail through the position and intensity changes of characteristic peaks, providing an important basis for the qualitative and quantitative analysis of sweat components. Through this spectrum, we can deeply understand the chemical composition of human sweat and its changing laws, providing scientific support for health monitoring and disease diagnosis.
[0165] Example 9
[0166] Based on Example 7, the signals collected by the silk fabric sensor of the present invention are classified and analyzed using a support vector machine (SVM). The working process of the support vector machine (SVM) is as follows: Fig.11 As shown, it mainly includes the following steps: data acquisition, data preprocessing, data segmentation, model training, model verification, classification prediction, and result output. Through the SVM algorithm flow chart, the whole process of sensor signal processing and classification can be seen, which provides technical support for biological stress detection and analysis.
Claims
1. A silk fabric sensor, characterized in that: The invention comprises placing an interpolation electrode (2) on a flexible substrate (1), the interpolation electrode (2) being covered with a silk fiber membrane (3), a sealing ring (4) being arranged above the silk fiber membrane (3) at the edge of the silk fiber membrane (3), and a packaging layer (5) being arranged above the sealing ring (4).
2. A method for preparing a silk fabric sensor, characterized in that: The silk fabric sensor as claimed in claim 1 is prepared by: Step 1, preparing a silk fiber membrane (3); Step 2, placing an interpolation electrode (2) on the flexible substrate (1), then covering the interpolation electrode (2) with the prepared silk fiber membrane (3), and ensuring that the silk fiber membrane (3) is in full contact with the interpolation electrode (2), and then placing a sealing ring (4) above the silk fiber membrane (3) at its edge, and finally encapsulating the whole above the sealing ring (4) to form an encapsulation layer (5).
3. The method for preparing the silk fabric sensor according to claim 2, characterized in that: The step 1 is specifically as follows: Step 1.1, pre-treating silk fibers; Step 1.2, depositing a gold seed layer on the surface of the pretreated silk fiber; Step 1.3, in situ growth of silver ions is performed on the gold seed layer, so that the silver ions grow on the gold seed layer to form silver nanoparticles and form a silk fiber membrane.
4. The method for preparing the silk fabric sensor according to claim 3, characterized in that: The step 1.1 is specifically as follows: taking out the natural silk fiber and soaking it in acetone for 20-30 minutes, then washing it thoroughly with deionized water until the washing liquid is clear; then soaking the washed silk fiber in alcohol for 20-30 minutes, then washing it thoroughly with deionized water again until the washing liquid is clear, and then drying it naturally at room temperature.
5. The method for preparing the silk fabric sensor according to claim 4, characterized in that: The step 1.2 is specifically as follows: Step 1.2.1, dissolving HAuCl4 in deionized water to prepare a 10-20 mM HAuCl solution, then immersing the silk fiber in the HAuCl solution and allowing it to stand at room temperature to allow the HAuCl to be evenly adsorbed on the surface of the silk fiber; Step 1.2.2, adding a reducing agent sodium borohydride solution dropwise to the chloroauric acid solution of step 1.2.1, and stirring for 1-3 minutes to allow gold nanoparticles to deposit on the surface of the silk fiber to form a gold seed layer; Step 1.2.3, taking out the silk fibers after the reaction in step 1.2.2, washing them with deionized water for several times until the washing liquid is clear and colorless, and then drying them at room temperature; Step 1.2.4, take out the dried silk fiber and repeat the steps 1.2.1-1.2.3 at least 3 times to obtain silk fiber with a gold seed layer deposited.
6. The method for preparing the silk fabric sensor according to claim 5, characterized in that: The concentration of the sodium borohydride solution in step 1.2.2 is 0.5-1M, and the volume ratio of the chloroauric acid solution to the sodium borohydride solution is 1.5:
1.
7. The method for preparing the silk fabric sensor according to claim 6, characterized in that: The step 1.3 is specifically as follows: Step 1.3.1, prepare a 10-20 mM silver nitrate solution and a 0.1 M ascorbic acid solution; Step 1.3.2, adding 5wt% PVP solution, acetonitrile, anhydrous ethanol, the silver nitrate solution and ascorbic acid solution prepared in step 1.3.1 to deionized water, and stirring to form a growth solution, wherein the volume ratio of the PVP solution, acetonitrile, anhydrous ethanol, silver nitrate solution, ascorbic acid solution and deionized water is 20:20:20:1.5:1:20; Step 1.3.3, placing the silk fibers treated in step 1.2 in a growth solution and subjecting them to magnetic stirring at -5 to -10°C for 10 to 30 minutes, so that the silver ions grow on the gold seed layer to form silver nanoparticles; Step 1.3.4, taking out the silk fibers after the reaction in step 1.3.3, washing them several times with deionized water until the washing liquid is clear, and then drying them at room temperature; Step 1.3.5, placing the dried silk fibers in a growth solution and repeating the process of steps 1.3.3-1.3.4 at least three times to obtain a silk fiber membrane.
8. The application of silk fabric sensor in muscle stress and strain detection and human biomolecule detection is characterized by: The silk fabric sensor prepared according to claim 7 is used to detect muscle stress and strain and human biomolecules.
9. The application of the silk fabric sensor according to claim 8 in muscle stress and strain detection and human biomolecule detection is characterized in that: When performing muscle stress and strain detection, the silk fabric sensor is attached to the position of the muscle to be detected and fixed with medical tape. The interpolation electrode (2) of the silk fabric sensor is connected to an electrochemical workstation to detect changes in biological stress and strain by monitoring different muscle movements.
10. The application of the silk fabric sensor according to claim 8 in muscle stress and strain detection and human biomolecule detection, characterized in that: When performing human biomolecule detection, the silk fiber membrane (3) in the silk fabric sensor is placed in a solution containing specific biomolecules, and then monitored using a handheld Raman spectrometer to identify the biomolecules therein.