Composite wires and their preparation methods
By introducing linear conductive reinforcing materials into the aluminum matrix and forming a conductive network, the problems of insufficient mechanical strength and conductivity of copper-clad aluminum composite wires are solved, and composite wires with both high mechanical properties and conductivity are prepared.
Patent Information
- Application Number
- CN202310477864.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-04-26
AI Technical Summary
Existing copper-clad aluminum composite conductors have limited mechanical strength, poor conductivity, and high cost, which restricts their application.
A conductive network is formed by oriented linear conductive reinforcing material within an aluminum matrix along the length of the composite conductor, and the interfacial bonding is enhanced through hot extrusion and hot drawing processes to prepare the composite conductor.
This technology improves the mechanical and electrical properties of composite conductors, making them lightweight and cost-effective for various applications.
Smart Images

Figure CN118866434B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of conductor technology, specifically to composite conductors and their preparation methods. Background Technology
[0002] Currently, pure copper wire has the best conductivity. However, pure copper wire has low mechanical strength, is prone to twisting and deformation, and is relatively expensive. Therefore, composite wires such as copper-clad aluminum have emerged. Copper-clad aluminum composite wires are popular due to their economic efficiency and lightweight nature. However, their mechanical strength is still limited, and because the aluminum matrix has poor conductivity, these composite wires rely mainly on the copper cladding layer to transmit current, significantly reducing their conductivity and greatly limiting their applications. Summary of the Invention
[0003] In view of this, this application provides a composite conductor that has both good mechanical properties and superior electrical conductivity, and is also lightweight and low in cost.
[0004] The first aspect of this application provides a composite conductor, including an inner core and a copper cladding layer; the inner core includes an aluminum matrix and linear conductive reinforcing materials disposed within the aluminum matrix, wherein at least 70% of the linear conductive reinforcing materials are oriented along the length direction of the composite conductor, and at least a portion of the linear conductive reinforcing materials are electrically connected to form a conductive network.
[0005] The aluminum matrix contains linear conductive reinforcing materials oriented along the composite conductor, which can improve the mechanical properties of the composite conductor, such as strength and ductility. Simultaneously, at least 70% of the linear conductive material is oriented along the length of the composite conductor, and the inner core also has linear conductive reinforcing materials electrically connected to form a conductive network, thus significantly improving the conductivity of the inner core. Therefore, the aforementioned composite conductor possesses both good mechanical properties and superior conductivity. Furthermore, based on the properties of aluminum, the aforementioned composite conductor also has the advantages of being lightweight and low-cost.
[0006] A second aspect of this application provides a method for preparing a composite conductor, comprising the following steps:
[0007] (1) In a protective atmosphere, the conductive reinforcing material raw material is mixed with aluminum particles so that the conductive reinforcing material raw material coats the surface of the aluminum particles to obtain the first raw material;
[0008] (2) The first raw material is filled into a copper sleeve and kept at a temperature of 400℃~550℃ and a pressure of 100MPa~400MPa to improve the interfacial bonding force between the conductive reinforcing material and the aluminum particles, thereby obtaining a composite wire blank.
[0009] (3) After the composite wire blank is kept at 400℃~550℃, it is hot extruded with an extrusion ratio of (9~25):1 to melt the aluminum particles to form an aluminum matrix and extend the conductive reinforcing material raw material along the length direction of the composite wire rod to form a linear conductive reinforcing material, thereby obtaining the composite wire rod.
[0010] (4) The composite conductor rod is subjected to multiple hot drawing processes to orient at least 70% of the linear conductive reinforcement material and to overlap at least some of the linear conductive reinforcement material to form a conductive network, thereby obtaining a composite conductor.
[0011] The above preparation method has simple steps, high process reliability, and can realize large-scale industrial production. Attached Figure Description
[0012] Figure 1 A schematic diagram illustrating the process principle of the composite conductor fabrication method provided in this application embodiment;
[0013] Figure 2 This is a scanning electron microscope (SEM) image of particles in the first raw material prepared in Example 1 of this application;
[0014] Figure 3 An optical photograph of the composite conductor obtained in Example 1 of this application;
[0015] Figure 4 Metallurgical microscope image of the cross-section of the composite wire prepared in Example 1;
[0016] Figure 5 This is a SEM image of the cross-section of the composite conductor obtained in Embodiment 1 of this application;
[0017] Figure 6 This is an SEM image of the first raw material obtained in Example 8 of this application;
[0018] Figure 7 An optical photograph of the composite wire rod prepared in Comparative Example 1 of this application;
[0019] Figure 8 This is a SEM image of the cross-section of the composite conductor prepared in Comparative Example 1 of this application. Detailed Implementation
[0020] This application provides a composite conductor, including an inner core and a copper cladding layer; wherein the inner core includes an aluminum matrix and linear conductive reinforcing material disposed within the aluminum matrix, at least 70% of the linear conductive reinforcing material is oriented along the length direction of the composite conductor, and at least a portion of the linear conductive reinforcing material is electrically connected to form a conductive network.
[0021] In the aforementioned core, linear conductive reinforcing materials oriented along the length direction of the composite conductor are distributed within the aluminum matrix. These linear conductive reinforcing materials can significantly improve the mechanical properties (e.g., strength and plasticity) of the core. Simultaneously, at least a portion of the conductive reinforcing materials are electrically connected to form a conductive network within the aluminum matrix. The electrical connection between the linear conductive reinforcing materials can exist in at least one of the following conditions (a) and (b): (a) a portion of the linear conductive reinforcing materials oriented along the length direction of the composite conductor has a small angle with the length direction of the composite conductor, and multiple oriented linear conductive reinforcing materials overlap each other to achieve electrical connection; (b) a portion of the linear conductive reinforcing materials is not oriented along the length direction of the composite conductor, and this portion of the linear conductive material acts as a "bridge" to achieve electrical connection between multiple oriented linear conductive reinforcing materials. Understandably, the conductive network formed by the linear conductive reinforcement material facilitates the plasticity of the aluminum matrix, and with at least 70% of the linear conductive reinforcement material oriented along the length of the composite conductor, it is more conducive to the rapid conduction of current along the length of the composite conductor. This results in higher plasticity for the composite conductor compared to pure copper conductors or general aluminum-reinforced core composite conductors, thus improving the fit of the composite conductor with other components during application (e.g., the fit of the composite conductor with the car body), allowing for further space optimization. Simultaneously, based on the conductivity of the conductive reinforcement material itself, the conductive network can significantly improve the conductivity of the core, enabling the composite conductor to possess both good mechanical properties and superior conductivity. Furthermore, based on the properties of aluminum, the composite conductor also has the advantages of being lightweight and low-cost. Moreover, a metallic diffusion effect can occur between copper and aluminum, resulting in excellent bonding at the copper / aluminum interface of the composite conductor, which also facilitates its application.
[0022] In this application, the orientation of the linear conductive reinforcing material along the length direction of the composite conductor specifically means that "the angle between the linear conductive reinforcing material and the length direction of the composite conductor is less than or equal to 45°".
[0023] In this application, "at least 70% of the linear conductive reinforcement material is oriented along the length direction of the composite conductor" means that "the composite conductor is sliced so that the slice exposes a cross-section of its core parallel to the length direction of the composite conductor. The cross-section of the core is observed under a scanning electron microscope (SEM). Based on the total amount of linear conductive material in a 5μm × 5μm field of view, the amount of linear conductive reinforcement material oriented along the length direction of the composite conductor is greater than or equal to 70%".
[0024] In this application, the proportion of linear conductive reinforcing material oriented along the length direction of the composite conductor can be 70%, 72%, 75%, 78%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 92%, 95%, 98%, 99%, etc.
[0025] In some embodiments of this application, at least 80% of the linear conductive reinforcing material is oriented along the length of the composite conductor. This facilitates faster current conduction along the length of the composite conductor.
[0026] In some embodiments of this application, the material of the aforementioned linear conductive reinforcing material includes, but is not limited to, at least one of graphene, carbon nanotubes, and carbon fibers. The carbon fibers can be carbon nanofibers or chopped carbon fibers. In some specific embodiments of this application, the aforementioned conductive reinforcing material is graphene. Graphene is an excellent reinforcing material, and it possesses excellent electrical and thermal conductivity, which can further improve the overall performance of the composite wire.
[0027] In some embodiments of this application, the mass percentage of the linear conductive reinforcing material is 5% to 50% based on the total weight of the inner core. Exemplarily, the mass percentage of the conductive reinforcing material in the inner core can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, etc. Controlling the content of the conductive reinforcing material within the above range results in a relatively larger number of cross-linking points in the conductive network, thereby increasing the conductivity of the conductive network and further enhancing the strength of the inner core, leading to better overall performance of the composite conductor.
[0028] In some embodiments of this application, the ratio of the radius of the inner core to the thickness of the copper cladding layer is 1:(0.1-10). Exemplary examples include ratios of 1:0.1, 1:0.2, 1:0.5, 1:0.8, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, and 1:10. This results in better performance in terms of conductivity, density, cost, and mechanical properties of the composite conductor, leading to a more balanced and superior performance across all aspects.
[0029] In this application, the aluminum substrate can be any aluminum metal material known in the art, and can be elemental aluminum or an aluminum alloy.
[0030] In this application, the copper coating can be any copper metal material known in the art, including elemental copper or copper alloy.
[0031] Accordingly, please see Figure 1This application also provides a method for preparing a composite conductor, which can be used to prepare the aforementioned composite conductor. The preparation method includes the following steps:
[0032] S01. In a protective atmosphere, the conductive reinforcing material raw material is mixed with aluminum particles so that the conductive reinforcing material raw material coats the surface of the aluminum particles to obtain the first raw material;
[0033] S02. The first raw material is filled into a copper sleeve and subjected to hot pressing densification treatment at a temperature of 400℃~550℃ and a pressure of 100MPa~400MPa to improve the interfacial bonding force between the conductive reinforcing material and the aluminum particles, thereby obtaining a composite wire blank. The hot pressing densification treatment in S02 can significantly improve the density of the first raw material, greatly strengthen the interfacial bonding force between the conductive reinforcing material and the aluminum particles, and fully compress the gaps between the aluminum particles whose surfaces are covered with conductive reinforcing material. This significantly reduces the risk of the conductive reinforcing material separating from the aluminum during hot drawing, which could result in the failure to form a conductive network or the presence of many defects in the conductive network. It can also avoid the risk of the composite wire blank breaking during hot drawing. For example, the temperature for hot-pressing densification can be 410℃, 420℃, 430℃, 440℃, 450℃, 460℃, 470℃, 480℃, 490℃, 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃, etc. If the temperature is too low, the densification degree will be insufficient; if the temperature is too high, the conductive reinforcing material will react with the aluminum matrix to form a third substance (e.g., Al4C3), severely damaging the performance of the composite wire. In some embodiments of this application, the conditions for the above-mentioned hot-pressing densification are: holding at 400℃~550℃ and 100MPa~400MPa for a first time. In some specific embodiments, the above-mentioned first time is 30min~60min.
[0034] In this application, the copper sleeve filled with the first raw material can be directly subjected to hot pressing densification treatment, without the need for any other pretreatment.
[0035] S03. After holding the composite wire blank under pressure at 400℃~550℃, hot extrusion is performed at an extrusion ratio of (9~25):1 to melt the aluminum particles to form an aluminum matrix, and to extend the conductive reinforcing material raw material along the length direction of the composite wire rod to form a linear conductive reinforcing material, thus obtaining a composite wire rod. Specifically, in the above process, the conductive reinforcing material raw material wrapped on the surface of the aluminum particles will extend along the length direction of the composite conductive rod to form a linear conductive reinforcing material. Specifically, in this process, taking graphene as an example, multiple sheet-like graphene particles will interact with each other to form a linear conductive reinforcing material. For example, the holding temperature before hot extrusion can be 410℃, 420℃, 430℃, 440℃, 450℃, 460℃, 470℃, 480℃, 490℃, 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, etc. If the temperature is too low, it will damage the interfacial properties between the conductive reinforcing material and the aluminum particle surface, causing the conductive reinforcing material raw material to fail to successfully form a conductive network subsequently. If the temperature is too high, the conductive reinforcing material will react with the aluminum matrix to generate a third substance. For example, the extrusion ratio can be 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, 21:1, 22:1, 23:1, 24:1, etc. In some specific embodiments, the composite conductor is subjected to a second voltage holding time at 400℃ to 550℃ for 30 min to 60 min.
[0036] The extrusion ratio mentioned above refers to the ratio of the cross-sectional area of the composite wire blank to the cross-sectional area of the composite wire rod after hot extrusion. If the extrusion ratio is too low, the conductive reinforcing material raw materials will agglomerate, ultimately failing to overlap and form a conductive network, or the surface of the composite wire rod will exhibit a fish-scale pattern, which is unfavorable for subsequent hot drawing. If the extrusion ratio is too high, the deformation will be too large, preventing the conductive reinforcing material from successfully forming a conductive network. In some specific embodiments, the extrusion ratio is (12-20):1. This is more conducive to the extension of the conductive reinforcing material to form linear conductive reinforcing material, and also facilitates the pre-orientation of the linear conductive reinforcing material, thereby facilitating its orientation and formation of a conductive network in subsequent processing. Simultaneously, it can further improve the smoothness of the composite wire rod surface, which is beneficial for subsequent hot drawing.
[0037] S04. The composite conductor rod is subjected to multiple hot drawing processes to orient at least 70% of the linear conductive reinforcement material and to overlap at least some of the linear conductive reinforcement material to form a conductive network, thereby obtaining a composite conductor. During the above hot extrusion and hot drawing processes, a metal diffusion reaction occurs at the interface between the aluminum matrix and the copper, forming a metallurgical bonding interface. Consequently, the interfacial bonding force between the core of the composite conductor and the copper cladding layer is strong, which is beneficial for the application of the composite conductor.
[0038] The above preparation method has simple steps, high process reliability, and can realize large-scale industrial production.
[0039] In some embodiments of this application, in step S01, mixing the conductive reinforcing material raw material with aluminum particles specifically involves placing the conductive reinforcing material raw material and aluminum particles in a solid-state mixing device and mixing them at a rotation speed of 100 rpm to 250 rpm. Exemplarily, the solid-state mixing device may be, but is not limited to, a planetary ball mill. In some embodiments, aluminum particles and conductive reinforcing material raw material are loaded into a ball mill jar, with a ball-to-material ratio of (10-15):1. In some specific embodiments, the conductive reinforcing material raw material and aluminum particles are placed in a ball mill jar and ball-milled at a rotation speed of 100 rpm to 250 rpm for 1 hour to 10 hours. Exemplarily, the rotation speed may be 100 rpm, 120 rpm, 150 rpm, 180 rpm, 200 rpm, 220 rpm, 230 rpm, 240 rpm, etc. If the rotation speed is too slow, the conductive reinforcing material raw material will not disperse well and will agglomerate severely, making it impossible to obtain aluminum particles wrapped by the conductive reinforcing material raw material; if the rotation speed is too fast, it will destroy the structure of the conductive reinforcing material raw material (e.g., graphene) or directly press the conductive reinforcing material raw material into the aluminum particles, which will also affect the formation of the conductive network in the composite wire.
[0040] In some embodiments of this application, in step S01, the D50 particle size of the aluminum particles is 800 μm to 1200 μm. Exemplarily, the D50 particle size of the aluminum particles can be 800 μm, 850 μm, 900 μm, 950 μm, 1000 μm, 1050 μm, 1100 μm, 1150 μm, 1200 μm, etc. This allows the reinforcing conductive material to be smoothly and uniformly coated on the surface of the aluminum particles, and greatly reduces the risk of poor bonding of the conductive reinforcing material due to excessively large aluminum particles during subsequent processing. In some embodiments of this application, the purity of the aluminum particles is greater than or equal to 99.9%.
[0041] In some embodiments of this application, the conductive reinforcing material raw materials include, but are not limited to, at least one of graphene, carbon nanotubes, and carbon fibers. The carbon fibers can be carbon nanofibers or chopped carbon fibers. In some specific embodiments of this application, the conductive reinforcing material raw material is graphene. Graphene is more easily interconnected in step S04 to form a conductive network, thereby significantly improving the yield; furthermore, given the excellent properties of graphene itself, the final composite wire has better overall performance.
[0042] In some embodiments of this application, the processing of the copper sleeve in S02 includes the following steps:
[0043] A copper alloy ingot with an aspect ratio of (5–10):1 is taken and machined into a sleeve shape to obtain a copper sleeve. The diameter of the copper alloy ingot is d, and the wall thickness of the copper sleeve is 0.1d–0.5d. This results in a high-quality copper cladding layer in the final composite conductor.
[0044] In some embodiments of this application, a pretreatment of the copper sleeve is performed before S02. Specifically, the inner surface of the copper sleeve is sequentially subjected to degreasing pickling, water washing, and drying.
[0045] In some embodiments of this application, during the hot extrusion process in step S03, the extrusion rate is 0.1 mm / s to 1 mm / s. Exemplarily, the extrusion rate can be 0.2 mm / s, 0.3 mm / s, 0.4 mm / s, 0.5 mm / s, 0.6 mm / s, 0.7 mm / s, 0.8 mm / s, 0.9 mm / s, etc. This results in a high degree of smoothness on the outer surface of the final composite wire, with a bright and scratch-free surface.
[0046] In some embodiments of this application, in step S04, the deformation of the composite conductor rod in a single-pass hot drawing process is 10% to 20%. For example, the deformation in a single-pass hot drawing process is 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, etc. This improves production efficiency while ensuring high quality of the final composite conductor, avoiding a fish-scale-like outer surface.
[0047] In some embodiments of this application, in step S04, after every two consecutive hot drawing processes, the composite conductor rod is annealed to remove internal stress from the material. In some embodiments of this application, the annealing conditions are: holding at 300°C to 500°C for 10 to 30 minutes.
[0048] The technical solution of this application will be further described in detail below with reference to several embodiments.
[0049] Example 1
[0050] (1) In a glove box filled with argon, conductive reinforcing material (specifically graphene with a purity of 99.9%) and aluminum particles (with a purity of 99.9% and a D50 particle size of 1000μm) with a mass ratio of 5:95 were loaded into a ball mill jar with a ball-to-material ratio of 10:1. The mixture was ball-milled at a ball milling speed of 100rpm for 10h to obtain the first raw material.
[0051] (2) Take an oxygen-free copper ingot blank with a length-to-diameter ratio of 5:1 and machine its interior to obtain an oxygen-free copper sleeve; wherein, the diameter of the oxygen-free copper ingot blank is 30mm, and the wall thickness of the oxygen-free copper sleeve is 3mm. The inner surface of the oxygen-free copper sleeve is sequentially degreasing, pickling, water washing, and drying.
[0052] The first raw material obtained in step (1) is filled into the oxygen-free copper sleeve and hot-pressed and densified at 500℃ and 300MPa for 30 minutes to obtain a composite wire blank.
[0053] (3) The above composite wire blank is kept at 450℃ for 30 minutes and hot extrusion is carried out at an extrusion ratio of 9:1. The extrusion speed is 1mm / s to obtain a composite wire rod with a diameter of 10mm.
[0054] (4) The composite conductor rod was subjected to 6 hot drawing processes, and the deformation of the composite conductor rod in each hot drawing process was 10%. After each two consecutive hot drawing processes, the rod was kept at 300℃ for 10 minutes to obtain the composite conductor.
[0055] Example 2
[0056] The only difference from Example 1 is that in step (1), the mass ratio of the conductive reinforcing material (specifically graphene) to the aluminum particles is 1:99.
[0057] Example 3
[0058] The only difference from Example 1 is that in step (1), the mass ratio of the conductive reinforcing material (specifically graphene) to the aluminum particles is 50:50.
[0059] Example 4
[0060] The only difference from Example 1 is that in step (2), the copper sleeve filled with the first raw material is kept at 400°C and 300MPa for 30 minutes.
[0061] Example 5
[0062] The only difference from Example 1 is that in step (2), the copper sleeve filled with the first raw material is kept at 550°C and 300MPa for 30 minutes.
[0063] Example 6
[0064] The difference from Example 1 is that in step (3), the above composite wire blank is kept at 450°C for 30 minutes and hot extruded at an extrusion ratio of 25:1 with an extrusion discharge speed of 1 mm / s to obtain a composite wire rod with a diameter of 6 mm.
[0065] Example 7
[0066] The difference from Example 1 is that in step (3), hot extrusion is performed with an extrusion ratio of 15:1.
[0067] Example 8
[0068] The difference from Example 1 is that in step (1), the ball milling speed is 50 rpm and the ball milling time is 0.5 h.
[0069] Example 9
[0070] The difference from Example 1 is that in step (4), the deformation of the composite conductive rod in a single hot drawing process is 25%.
[0071] To highlight the beneficial effects of the embodiments of this application, the following comparative examples are provided.
[0072] Comparative Example 1
[0073] The difference from Example 1 is that in step (3), the above composite wire blank is held at 450°C for 30 minutes and hot extrusion is performed with an extrusion ratio of 3:1. The extrusion speed is 1 mm / s, and a composite wire rod with a diameter of 17.3 mm is obtained.
[0074] Comparative Example 2
[0075] The difference from Example 1 is that in step (2), the above composite wire is kept at 350°C and 200MPa for 20 minutes.
[0076] Comparative Example 3
[0077] The only difference from Example 1 is that step (1) is omitted, and the aluminum particles from Example 1 are directly added to the copper sleeve from Example 1.
[0078] Comparative Example 4
[0079] The only difference from Example 1 is that step (1) is omitted, and in step (2), oxygen-free copper is directly subjected to hot pressing densification treatment to obtain pure copper wire.
[0080] Performance testing
[0081] (1) Conductivity test: Refer to GB / T11007-2008 standard for conductivity meter test method.
[0082] (2) Tensile strength test: Refer to GB / T228.1-2010 Metallic materials, tensile testing, part 1: room temperature test method.
[0083] (3) Elongation test: Refer to GB / T228.1-2010 Metallic materials, tensile testing, part 1: room temperature test method.
[0084] (4) Density test: Refer to GB / T1423-1996 standard for testing the density of precious metals and their alloys.
[0085] (5) Morphology test: The first raw material was observed under a scanning electron microscope. SEM images of the first raw material in some embodiments are shown below. Figure 2 , Figure 6 As shown.
[0086] The cross-section of the composite conductor (obtained by cutting the composite conductor with a plane parallel to its length) was observed under a scanning electron microscope; Example 1: SEM image of the composite conductor cross-section as shown below. Figure 5 As shown, the cross-sectional SEM image of the composite conductor in Example 8 is as follows. Figure 8 As shown.
[0087] The cross-section of the composite conductor (a cross-section perpendicular to the length of the composite conductor) was observed under a metallographic microscope. Example 1: SEM image of the cross-section of the composite conductor is shown below. Figure 4 As shown.
[0088] The morphology of the composite wire and composite wire rod was observed. An optical photograph of the composite wire obtained in Example 1 is shown below. Figure 3 As shown; an optical photograph of the composite wire rod prepared in Comparative Example 1 is shown. Figure 7 As shown.
[0089] Table 1
[0090]
[0091] Please refer to the data in Table 1. Comparing the data of Example 1 and Comparative Example 3, it can be found that the addition of the conductor reinforcement material has almost no effect on the density of the composite conductor, allowing the composite conductor to maintain a density equivalent to that of an all-aluminum core composite conductor, resulting in a lightweight composite conductor. Simultaneously, the conductive network formed after the linear conductive reinforcement material is oriented not only to improve the conductivity of the composite conductor but also to a certain extent to improve its mechanical properties, making it more suitable for use. Comparing the data of Example 1 and Comparative Examples 1 and 2, it can be found that when the steps and parameters in the composite conductor preparation process do not conform to the limitations of this application, the conductivity of the resulting composite conductor is poor. Specifically, the hot extrusion ratio in Comparative Example 1 was too low, leading to agglomeration of the conductive reinforcement material raw materials (see [link to Comparative Example 1]). Figure 8 This results in low conductivity of the composite wire. In Comparative Example 2, the temperature and pressure used in the thermal densification process in step (2) were too low, resulting in low density of the first raw material. Consequently, the conductive reinforcing material could not form a conductive network smoothly or the formed conductive network had many defects, leading to low conductivity of the composite wire.
[0092] The above description is an exemplary embodiment of this application. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principles of this application, and these improvements and modifications are also considered to be within the scope of protection of this application.
Claims
1. A composite conductor, characterized in that, The composite conductor includes an inner core and a copper cladding layer; wherein, the inner core includes an aluminum matrix and a linear conductive reinforcing material disposed within the aluminum matrix, and the mass percentage of the conductive reinforcing material is 5% to 50% based on the total mass of the inner core; At least 70% of the linear conductive reinforcing material is oriented along the length of the composite conductor, and at least a portion of the linear conductive reinforcing materials are electrically connected to form a conductive network; the material of the linear conductive reinforcing material includes at least one of graphene, carbon nanotubes, and carbon fibers.
2. The composite conductor according to claim 1, characterized in that, At least 80% of the linear conductive reinforcement material is oriented along the length of the composite conductor.
3. A method for preparing a composite conductor, characterized in that, Includes the following steps: (1) In a protective atmosphere, a conductive reinforcing material raw material is mixed with aluminum particles to coat the surface of the aluminum particles, thereby obtaining a first raw material; wherein, based on the mass of the first raw material, the mass percentage of the conductive reinforcing material is 5% to 50%; the material of the conductive reinforcing material includes at least one of graphene, carbon nanotubes and carbon fibers; the D50 particle size of the aluminum particles is 800 μm to 1200 μm; (2) The first raw material is filled into a copper sleeve and kept at a temperature of 400°C to 550°C and a pressure of 100MPa to 400MPa to improve the interfacial bonding force between the conductive reinforcing material and the aluminum particles, thereby obtaining a composite wire blank. (3) After the composite wire blank is kept at 400°C to 550°C, it is hot extruded at an extrusion ratio of (9 to 25): 1 to melt the aluminum particles to form an aluminum matrix and extend the conductive reinforcing material along the length of the composite wire blank to form a linear conductive reinforcing material, thereby obtaining a composite wire rod. (4) The composite conductor rod is subjected to multiple hot drawing processes to orient at least 70% of the linear conductive reinforcement material and to overlap at least some of the linear conductive reinforcement material to form a conductive network, thereby obtaining a composite conductor.
4. The preparation method according to claim 3, characterized in that, In step (1), the mixing of the conductive reinforcing material raw material and the aluminum particles specifically involves placing the conductive reinforcing material raw material and the aluminum particles in a solid-phase mixing device and mixing them at a speed of 100 rpm to 250 rpm.
5. The preparation method according to any one of claims 3-4, characterized in that, In step (2), the copper sleeve filled with the first raw material is kept warm and pressurized at a temperature of 400°C to 550°C and a pressure of 100MPa to 400MPa.
6. The preparation method according to claim 3, characterized in that, In step (3), the extrusion ratio is (12~20):
1.
7. The preparation method according to claim 3 or 6, characterized in that, In step (4), the deformation of the composite wire rod is 10%~20% in the single-pass hot drawing process.
Citation Information
Patent Citations
Graphene copper clad aluminum alloy flat wire and preparation method thereof
CN108538452A