Surface passivation technology for improving electrochemical performance of niobium diboride

Optimizing the NbB2 surface through atomic-level surface passivation technology solves the problem of limited catalytic performance of niobium diboride in lithium-sulfur batteries, achieves effective anchoring of polysulfide intermediates and improves catalytic activity, and prolongs the life of lithium-sulfur batteries. service life.

CN118867239APending Publication Date: 2024-10-29XUZHOU NORMAL UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410815956.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The catalytic performance of niobium diboride in lithium-sulfur batteries is limited by the super strong adsorption capacity of sulfur species on the surface, resulting in the inability to desorb sulfur and resulting in battery performance degradation. Existing technology cannot effectively solve this problem.

Method used

Adopting atomic level surface passivation technology, by mixing Nb2O5, boron powder, passivation layer source and salt for high-temperature sintering treatment, the chemical bond energy and morphology of the NbB2 surface are optimized, and different passivation layer sources and salt ratios are used to adjust passivation The effect is to obtain optimized NbB2 nanoparticle materials.

Benefits of technology

Effectively anchor polysulfide intermediates, improve catalytic activity, enhance the redox kinetics of LiPSs, extend the service life of lithium-sulfur batteries, and improve battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867239A_ABST
    Figure CN118867239A_ABST
Patent Text Reader

Abstract

Niobium diboride (NbB2) has unique physicochemical characteristics and electrochemical properties, the targeted design and reasonable application of the NbB2 are effective ways for relieving the shuttle effect of the lithium-sulfur battery and improving reaction kinetics and reversibility, and the development momentality is rapid in recent years. However, the high surface adsorption energy of the material causes the material to be poisoned in the electrochemical reaction process. The invention relates to an atomic level surface passivation technology for passivating the NbB2 surface, moderately reducing the adsorption of sulfur-containing species, and avoiding NbB2 poisoning, thereby improving the battery performance. The implementation method comprises the following steps: uniformly mixing Nb2O5, boron powder (B), a passivation layer source, sodium chloride and potassium chloride by adopting a molten salt method, fully grinding, sintering at high temperature, cooling, dissolving with distilled water, stirring to remove salt, washing and drying to obtain the atomic-level carbon, oxygen or transition metal passivated NbB2 nano-particles. The surface-passivated NbB2 electrocatalyst prepared by the technology can effectively improve the cycling stability and the energy density of a lithium-sulfur battery.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Technical field: The present invention belongs to the field of nanomaterial science, and specifically relates to an atomic-level surface passivation technology for improving the electrocatalytic performance of niobium diboride. Background technology:

[0002] Lithium-sulfur (Li-S) batteries are strong contenders for next-generation energy storage systems, characterized by abundant sulfur resources, strong environmental sustainability, and large specific capacity. However, the practical implementation of energy storage systems using Li-S batteries still faces challenges and limitations, with soluble polysulfide (LiPSs) intermediates causing a "shuttle effect" that leads to capacity decay. To promote the further development of lithium-sulfur batteries, efficient catalysts are needed to accelerate the conversion of LiPSs and inhibit their shuttling. Metallic niobium borides are a class of intermetallic compounds that have unlimited potential due to their metallic properties due to metallic bonding. Compared with other transition metal compounds (such as sulfides, nitrides, and phosphides), the diversity of crystal structures and chemical bond types possessed by interstitial niobium borides leads to their different physical and chemical properties, including high conductivity and special catalytic ability. Therefore, these borides have a wide range of applications in various fields such as superconductivity, development of superhard materials, magnetocaloric effect, electronics, catalysis, and corrosion resistance. For example, niobium boride (NbB2) with special physical and chemical properties can enhance the redox kinetics of LiPSs. Recent studies have shown that NbB2 has potential catalytic performance in Li-S batteries, where both Nb and electron-deficient B can adsorb LiPSs through BS and Nb-S bonds, greatly enriching the anchoring and catalytic active sites. However, the NbB2 surface exhibits a super strong adsorption capacity for S species, especially the Nb end (>12eV), which causes S to be firmly adsorbed on its surface and unable to desorb (dead sulfur), causing NbB2 poisoning and battery performance degradation. However, this problem has neither received much attention nor been resolved. Summary of the invention:

[0003] Based on the above problems, this paper proposes an atomic-level surface passivation technology to improve the electrocatalytic performance of niobium diboride. The technology includes the following steps:

[0004] (1) Nb2O5, boron powder (B), passivation layer source, sodium chloride and potassium chloride are mixed evenly and ground thoroughly;

[0005] (2) The material obtained in step (1) is transferred to a tube furnace for high-temperature sintering treatment for 1-48 hours, washed with hot deionized water and stirred for 1-24 hours to remove the remaining salt, washed with water and ethanol 3-7 times, filtered, and dried overnight to obtain atomic-level passivated NbB2 nanoparticle material.

[0006] Preferably, in step (1), the salt used may be one or more of sodium chloride, potassium chloride, calcium chloride, magnesium chloride and aluminum chloride.

[0007] Preferably, in step (1), the mass ratio of Nb2O5 to boron powder (B) is 1:1 to 1:4.

[0008] Preferably, in step (1), the mass ratio of the two salts is 1:1 to 1:3.

[0009] Preferably, in step (1), if NbB2 passivated with a carbon atom layer is obtained, the passivation layer source used may be one or more of urea, melamine, glucose, and phytic acid.

[0010] Preferably, in step (1), if NbB2 passivated with transition metal atoms is obtained, the passivation layer source used may be one or more of metal nitrates, metal chlorides, metal carbonates, and metal acetates.

[0011] Preferably, in step (1), if non-metal atom passivated NbB2 is obtained, there is no need to add a passivation layer source in claim (1), but oxygen is introduced or one or more of sulfuric acid and hydrofluoric acid are added after desalination.

[0012] In summary, the present invention discloses an atomic-level surface passivation technology for improving the electrocatalytic performance of niobium diboride, which can effectively anchor LiPSs. At the same time, by adjusting the mass ratio of different Nb2O5 and boron powder (B) and the mass ratio of two different salts, the chemical bond binding energy on the NbB2 surface can be optimized. The surface morphology of nano NbB2 particles can be optimized by adjusting the temperature of high-temperature sintering; the passivation effect can be optimized by adjusting the type of passivation layer source added, thereby improving the surface passivation of NbB2. Description of the drawings:

[0013] Figure 1 The decomposition process of O2 on the NbB2 catalyst surface obtained in Example 1 of the present invention, (a) the decomposition process of O2 on the Nb surface and (b) the decomposition process of O2 on the B surface. Nb, B and O atoms are represented by cyan, pink and red balls, respectively. (c) The corresponding structure of S8 adsorbed on the Nb-O and (d) BO surface systems changes with time, where Nb, B and S are represented by blue, pink and yellow balls, respectively.

[0014] Figure 2 (a) AC TEM image of Example 1 of the present invention and the corresponding NbB2 mapping diagram. B, Nb and O atoms are represented by blue, orange and yellow, respectively. (b) B1s and Nb 3D XPS spectra of NbB2. (ce) Raman spectrum of NbB2 and Raman mapping of BO and Nb-O bonds. (fh) Li 1s, B1s and Nb 3d XPS of NbB2 under different charge and discharge states.

[0015] Figure 3 The polysulfide lithium (Li2S n ) adsorption configuration on O2-NbB2.

[0016] Figure 4 This is the performance diagram of lithium-sulfur battery of NbB2 / rGO / PP at 5C current density. Specific implementation method:

[0017] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and accompanying drawings:

[0018] Embodiment 1:

[0019] This embodiment provides an atomic-level surface passivation technology for improving the electrocatalytic performance of niobium diboride, which specifically includes the following steps:

[0020] (1) Place 0.14 g Nb2O5, 0.044 g boron powder (mass ratio is 1:3) (B), 0.8 g sodium chloride and 1.03 g potassium chloride (mass ratio is 1:1) into a mortar and grind thoroughly for 30 min.

[0021] (2) Heat at 950°C for 1.5 h under nitrogen atmosphere. After cooling, stir the black powder in hot water for 12 h to remove the remaining salt, and introduce oxygen for 10 min. Then wash with water and ethanol several times, filter, and dry overnight.

[0022] Embodiment 2:

[0023] An atomic level surface passivation technique for improving the electrocatalytic performance of niobium diboride comprises the following implementation steps:

[0024] (1) 0.14 g Nb2O5, 0.035 g boron powder (B) (mass ratio of 1:4), 0.8 g sodium chloride and 1.6 g potassium chloride (mass ratio of 1:2), and 0.1 g phytic acid were placed in a mortar and ground thoroughly for 30 min.

[0025] (2) Heat at 800°C for 1 h under argon atmosphere. After cooling, stir the black powder in hot water for 12 h to remove the remaining salt. Then wash it with water and ethanol several times, filter it, and dry it overnight.

[0026] Embodiment 3:

[0027] This embodiment is similar to embodiment 2, except that the phytic acid in step 1 is replaced with melamine, and the other conditions remain unchanged.

[0028] Embodiment 4:

[0029] This embodiment is similar to embodiment 2, except that the phytic acid in step 1 is replaced with copper nitrate, and the other conditions remain unchanged.

[0030] The following are the results of characterizing and testing Example 1:

[0031] Figure 1 HAADF diagram of NbB2 and the corresponding elemental mapping diagram. B, Nb and O atoms are represented by blue, orange and yellow, respectively.

[0032] Figure 2 Raman spectrum of NbB2 and Raman mapping of BO and Nb-O bonds.

[0033] Figure 3 Lithium polysulfide (Li2S n ) adsorption configuration on O2-NbB2.

[0034] Figure 4 The performance of lithium-sulfur battery of NbB2 / rGO / PP at 5C current density.

Claims

1. An atomic level surface passivation technology for improving the electrocatalytic performance of niobium diboride, characterized in that: Due to the presence of the atomic-level passivation layer on the surface, the adsorption capacity of NbB2 for sulfur-containing species is moderately reduced, avoiding poisoning, so that the battery exhibits high performance.

2. This patent involves a technology to achieve atomic-level passivation of the surface of NbB2 to prevent it from being poisoned, which can effectively improve the performance of lithium-sulfur batteries as an electrocatalyst. The steps of preparing surface passivated NbB2 using this technology include: Step 1: Mix Nb2O5, boron powder (B), passivation layer source, sodium chloride and potassium chloride evenly and grind them thoroughly; Step 2: After high-temperature sintering, cool down, dissolve and stir with hot distilled water for 12 hours to remove salt, wash and dry with ethanol and water, and filter to obtain atomic-level passivated NbB2 nanoparticles.

3. The atomic level surface passivation technology for improving the electrocatalytic performance of niobium diboride as claimed in claim 2, characterized in that: In step 1, the salt used can be two of sodium chloride, potassium chloride, calcium chloride, magnesium chloride and aluminum chloride.

4. The atomic level surface passivation technology for improving the electrocatalytic performance of niobium diboride according to claim 2, characterized in that: In step 1, the mass ratio of Nb2O5 and boron powder (B) is 1:(1-4).

5. The atomic level surface passivation technology for improving the electrocatalytic performance of niobium diboride as claimed in claim 2, characterized in that: In step 1, the mass ratio of the two salts is 1:(1-3).

6. The atomic level surface passivation technology for improving the electrocatalytic performance of niobium diboride as claimed in claim 1, characterized in that: In step 2, if NbB2 passivated with a C atomic layer is obtained, the passivation layer source used can be one of urea, melamine, glucose, and phytic acid.

7. The atomic level surface passivation technology for improving the electrocatalytic performance of niobium diboride as claimed in claim 1, characterized in that: In step 2, if NbB2 passivated with transition metal atoms is obtained, the passivation layer source used can be one of metal nitrates, metal chlorides, metal carbonates, and metal acetates.

8. The atomic level surface passivation technology for improving the electrocatalytic performance of niobium diboride as claimed in claim 1, characterized in that: In step 2, if NbB2 passivated with non-metallic atoms is obtained, there is no need to add a passivation layer source in claim (1), but instead O2 is introduced or one of sulfuric acid and hydrofluoric acid is added after desalination.

Citation Information

Cited By

  • Preparation method and application of niobium boride-niobium oxide complex phase three-dimensional material