NCO-terminated prepolymers for coating applications

By optimizing the functional groups and molecular structure in the NCO-terminated prepolymer, the existing problems of non-drying and insufficient solvent resistance of NCO-terminated prepolymers when cured with commercially available polyols are solved, and high-performance coatings are realized The cured composition improves the hardness and solvent resistance of the coating.

CN118871491APending Publication Date: 2024-10-29COVESTRO DEUTSCHLAND AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027297.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-16
Filing Date
2023-03-15
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing NCO-terminated prepolymers are difficult to produce suitable coatings when cured with commercially available standard polyols, and have non-drying properties and limited solvent resistance.

Method used

An NCO-terminated prepolymer in general formula (I) was developed. By removing specific functional groups from the reaction of polyol and diisocyanate, a prepolymer with specific NCO content, number average molecular weight and polydispersity was prepared, and Distillation at high temperature removes excess monomer, reduces monomer diisocyanate content, and improves the solvent resistance and chemical resistance of the cured composition.

Benefits of technology

It is possible to use standard commercially available polyols to formulate curable compositions, maintain excellent physical and chemical properties, improve the hardness and solvent resistance of the coating, and ensure the stability and performance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005040608760000011
    Figure BDA0005040608760000011
  • Figure BDA0005040608760000051
    Figure BDA0005040608760000051
  • Figure BDA0005040608760000134
    Figure BDA0005040608760000134
Patent Text Reader

Abstract

The invention relates to an NCO-terminated prepolymer for coating applications, to a method for producing the NCO-terminated prepolymer according to the invention, and to the use of the NCO-terminated prepolymer according to the invention. The invention further relates to a two-component system comprising component A) comprising at least one NCO-terminated prepolymer according to the invention and component B) comprising at least one compound containing at least one Zerewitinoff active group. In addition, the present invention relates to a method for curing the composition on a substrate and a cured article.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to an NCO-terminated prepolymer for coating applications, to a method for preparing the NCO-terminated prepolymer according to the invention, and to the use of the NCO-terminated prepolymer according to the invention. The present invention further relates to a two-component system comprising component A) and component B), wherein component A) comprises at least the NCO-terminated prepolymer according to the invention and component B) comprises at least one compound containing at least one Zerevdinov-active group. Furthermore, the present invention relates to a method for curing a composition on a substrate and to the cured article.

[0002] It is known that NCO-terminated prepolymers can be used as curing components in polyurethane coatings or coating systems. These prepolymers are usually obtained by reacting polyols with diisocyanates or polyisocyanates. As curing components, the prepolymers are subsequently reacted in a coating or coating system with further polyols, for example with polyacrylate polyols, to produce the corresponding polyurethanes. Depending on the desired application, for example original equipment manufacturer (OEM) coating processes or manual coating applications in the refinishing industry, the requirements for the coating composition used can vary greatly.

[0003] WO 2016 / 116376 A1 describes isocyanate-functional polyester prepolymers composed of a combination of branched polyesters and caprolactone polyesters, which have low viscosity and are simultaneously crystallization-stable at temperatures above 5° C. and have high elasticity. However, these prepolymers do not produce suitable coatings when cured with commercially available standard polyols. In particular, these formulations do not dry and have limited solvent resistance.

[0004] It was therefore an object of the present invention to provide an NCO-terminated prepolymer which enables the formulation of curable compositions using standard commercial polyols as binders while retaining the excellent physical and chemical properties of the coatings obtained.

[0005] The inventors have surprisingly found that the following aspects of the present invention can overcome the above-mentioned deficiencies:

[0006] The present invention relates to an NCO-terminated prepolymer for coating applications, preferably for manual coating applications, having the general formula (I),

[0007]

[0008] where P, Q and p are defined as follows

[0009] P is each independently at least one organic group obtained by removing a hydroxyl group from a polyol unit,

[0010] Q is each independently at least one organic group obtained by removing an isocyanate group from a monomeric diisocyanate unit and / or at least one organic group obtained by removing an isocyanate group from a uretdione unit having two isocyanate groups, and

[0011] p is each independently a number ≥ 2.0, and

[0012] The NCO-terminated prepolymer has

[0013] a NCO content of ≥6.5 wt. % to ≤12.0 wt. %, based on the total solids content of the NCO-terminated prepolymer, and

[0014] a content of ≤17 wt. % of oligomers having a number average molecular weight ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, and

[0015] a content of monomeric diisocyanates of <0.5% by weight, based on the total solids content of the NCO-terminated prepolymer, and

[0016] Polydispersity a ≥ 2.0.

[0017] In the present invention, any numerical range described herein is intended to include all sub-ranges contained therein. For example, a range of "1 to 10" is intended to include all sub-ranges between the minimum value 1 and the maximum value 10 (and including 1 and 10), i.e., having a minimum value equal to or greater than 1 and a maximum value equal to or less than 10.

[0018] In the context of the present invention, "unit" means that the structural unit present in the general formula (I) is derived from the reactive compound described below. For example, when a diisocyanate is converted using a diol or polyol, one isocyanate group and one hydroxyl group form a carbamate group. However, the remaining compounds used (such as the six methyl groups of hexamethylene diisocyanate) remain unchanged. Therefore, in the present invention, "unit" is understood to mean the part of the compound that does not participate in the reaction and the functional group (such as a hydroxyl group or an isocyanate group) that reacts to form the carbamate group shown in the general formula (I). In the context of the present invention, the corresponding unit is always derived from the compound used in the synthesis.

[0019] In the context of the present invention, "each independently" means that if the corresponding units in the general formula (I) are multiple, these units are identical or different and are selected from the group of possible units. According to the present invention, mixtures of compounds of the general formula (I) may also be present in which different possible units are present in a single molecule.

[0020] The prepolymers of the general formula (I) according to the invention are NCO-terminated. In the present invention, the term "NCO-terminated" means that the functional end groups present are essentially isocyanate groups. The term "essentially" in this respect means that preferably at least 80 mol %, more preferably at least 90 mol %, and most preferably ≥ 99 mol % to 100 mol % of the functional end groups present in the NCO-terminated prepolymer are isocyanate groups, also referred to herein as NCO groups.

[0021] In the present invention, the term "polymer" refers to a compound formed by linking together a plurality of monomers (i.e. more than two monomers) of the same or different kinds via covalent bonding during a chemical reaction, wherein the resulting polymers may differ in their degree of polymerization, molecular weight distribution and chain length. Thus, a polymer according to the present invention is a compound comprising at least one repeating unit in its molecular structure, which is incorporated into the polymer structure during the polymer synthesis process by repeatedly linking together monomers via covalent bonds to form the polymer structure.

[0022] The term "polymer" includes homopolymers, copolymers, block copolymers and oligomers.

[0023] In the present invention, "prepolymer" is a polymer with reactive groups. Similar to the definition of the term "polymer", the molecular structure of the prepolymer is formed by repeatedly connecting more than two monomers of the same or different types together. The prepolymer can participate in the subsequent polymer formation, which has a higher molecular weight than the prepolymer. The term "prepolymer" covers polymers that can chemically react via at least one of its reactive groups to form repeating units of (preferably cross-linked) polymers. Therefore, the term "prepolymer" also covers self-crosslinking polymers with at least two different types of reactive groups, wherein the groups can chemically react between themselves so that the prepolymer molecules can be cross-linked. The number average molecular weight is preferably at least 900 g / mol, more preferably at least 1,000 g / mol.

[0024] According to the invention, if there is no other provision, the average molecular weight is defined as the number average molecular weight M n As the molecular weight of the polymer, the number average molecular weight M is used. n . M n The determination was carried out at 23° C. with tetrahydrofuran as solvent via gel permeation chromatography (GPC). The measurement was carried out as described in DIN 55672-1:2016-03 “Gelpermeationschromatographie, Teil1-Tetrahydrofuran als Elutionsmittel”

[0025] According to the invention, the content of oligomers with a number average molecular weight ≤ 1000 g / mol is determined using the aforementioned GPC method. The proportion is taken from the chromatogram expressed in area % determined with software support and is approximately equal to the proportion expressed in weight %.

[0026] The content of monomeric diisocyanates is determined in accordance with DIN EN ISO 10283:2007-11 by gas chromatography using an internal standard and is preferably <0.3% by weight, based on the total solids content of the NCO-terminated prepolymer.

[0027] The NCO content is determined by titration in accordance with DIN EN ISO 11909:2007-05.

[0028] According to the invention, the polydispersity is determined according to DIN 55672-1:2016-03.

[0029] An "organic compound" contains at least one moiety comprising a carbon-hydrogen covalent bond.

[0030] According to this invention, the term "aliphatic" is defined as a saturated or unsaturated non-aromatic hydrocarbon group.

[0031] According to this invention, the term "araliphatic" is defined as a hydrocarbyl moiety consisting of a non-aromatic and saturated or unsaturated hydrocarbyl group directly bonded to an aromatic moiety.

[0032] According to the invention, the term "alicyclic" or "cycloaliphatic" is a non-aromatic, optionally substituted carbocyclic or heterocyclic compound or moiety (such as, for example, cycloalkanes, cycloalkenes or oxacycloalkanes, thiacycloalkanes, azacycloalkanes or thiazazacycloalkanes). Specific examples are cyclohexyl, cyclopentyl and their N-heterocyclic derivatives or O-heterocyclic derivatives, such as, for example, pyrimidine, pyrazine, tetrahydropyran or tetrahydrofuran.

[0033] According to the invention, the term "polyol unit P" may include other intramolecular functional groups, such as, for example, carbamate groups. Independent of these intramolecular functional groups that may optionally be present, all "polyol units P" meet the definition of the general formula (I) of the present invention. These intramolecular functional groups can be formed, for example, by feasible chain extension during the prepolymer synthesis process.

[0034] According to the invention, the NCO-terminated prepolymers of the general formula (I) contain carbamate groups as intramolecular functional groups and substantially do not contain other functional groups derived from NCO groups, such as, for example, isocyanurate groups. "Substantially" in this context means that, in addition to the carbamate groups, other functional groups are contained only in very small amounts, which other functional groups may be unavoidable, for example, during the synthesis process. Preferably, such other functional groups are present only in an amount of ≤5 mol %, more preferably ≤2 mol %, and most preferably ≤0.5 mol %, based on the amount of carbamate groups in the NCO-terminated prepolymer. The same definitions and preferred embodiments apply to the NCO-terminated prepolymers obtained or obtainable by the process of the invention.

[0035] The mol% content of the carbamate groups contained in the general formula (I) and not substantially in the other intramolecular functional groups mentioned above (e.g. "isocyanurate groups") is the decoupling of protons. 13 The integral of the C-NMR spectrum was calculated based on the solution in CDCl 3 In the case of the NCO-terminated prepolymer of 1,6-diisocyanatohexane (HDI) in , the individual structural elements have the following chemical shifts (in ppm): isocyanurate: 148.4 and urethane: 156.3.

[0036] In a first preferred embodiment, the NCO-terminated prepolymers of the general formula (I) according to the invention are characterized in that the content of oligomers having a number average molecular weight of ≤1000 g / mol is ≥0.5% by weight to ≤17% by weight, preferably ≥1.0% by weight to ≤14% by weight, and most preferably ≥1.5% by weight to ≤10% by weight, based on the total solids content of the NCO-terminated prepolymer. This has the advantage that the solvent resistance and chemical resistance of the cured composition are further increased.

[0037] In a preferred embodiment, the NCO-terminated prepolymer of the general formula (I) according to the invention is characterized in that the NCO-terminated prepolymer has an NCO content of ≥7.5 wt. % to ≤11.0 wt. %. This has the advantage that the hardness of the coating is still sufficient while minimizing the number of reactive groups.

[0038] In principle, the NCO-terminated prepolymers of the general formula (I) according to the invention can have any molecular weight known to the person skilled in the art. In a preferred embodiment, the NCO-terminated prepolymers of the general formula (I) according to the invention are characterized in that the NCO-terminated prepolymers have a number average molecular weight Mn of ≥1700 g / mol, preferably ≥1700 g / mol to ≤3500 g / mol, more preferably ≥1700 g / mol to ≤3100 g / mol. The average molecular weight Mn is determined according to the above-mentioned method.

[0039] In a preferred embodiment, the NCO-terminated prepolymers of the general formula (I) according to the invention are characterized in that the NCO-terminated prepolymers have an average NCO functionality of >2.0, preferably >2.7. The functionality is calculated using the following formula:

[0040]

[0041] Typically, the unit Q in the NCO-terminated prepolymer of the general formula (I) of the present invention is at least one aliphatic, cycloaliphatic, araliphatic and / or aromatic group obtained by removing an isocyanate group from a monomeric diisocyanate unit and / or at least one organic group obtained by removing an isocyanate group from a uretdione unit having two isocyanate groups.

[0042] Suitable monomeric diisocyanates OCN-Q-NCO have aliphatically, cycloaliphatically, araliphatically and / or aromatically bound isocyanate groups.The monomeric diisocyanates can be prepared by any desired process, for example by phosgenation or by a phosgene-free route, for example by carbamate cleavage.

[0043] For example, these monomeric diisocyanates (hereinafter also referred to as starting diisocyanates) are those with a molecular weight range of 168 g / mol to 400 g / mol, such as 1,4-butanediisocyanate, 1,5-diisocyanatopentane (PDI), 1,5-diisocyanato-2,2-dimethylpentane, 1,6-diisocyanatohexane (HDI), 2,2,4- or 2,4,4-trimethyl-1,6-diisocyanatohexane, 1,8-diisocyanatooctane, 1,9-diisocyanatononane, 1,10-diisocyanatodecane, 1,3- and 1,4-diisocyanatohexane. Cyclohexane, 1,4-diisocyanato-3,3,5-trimethylcyclohexane, 1,3-diisocyanato-2-methylcyclohexane, 1,3-diisocyanato-4-methylcyclohexane, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate; IPDI), 1-isocyanato-1-methyl-4(3)-isocyanatomethylcyclohexane, 2,4'- and 4,4'-diisocyanatodicyclohexylmethane (H12-MDI), 1,3- and 1,4-bis(isocyanatomethyl)cyclohexane, 4,4'-diisocyanato- 3,3'-dimethyldicyclohexylmethane, 4,4'-diisocyanato-3,3',5,5'-tetramethyldicyclohexylmethane, 4,4'-diisocyanato-1,1'-bis(cyclohexyl), 4,4'-diisocyanato-3,3'-dimethyl-1,1'-bis(cyclohexyl), 4,4'-diisocyanato-2,2',5,5'-tetramethyl-1,1'-bis(cyclohexyl), 1,8-diisocyanato-p-methane, 1,3-diisocyanato-adamantane, 1,3-dimethyl-5 ,7-diisocyanatoadamantane, 1,3- and 1,4-bis(isocyanatomethyl)benzene (XDI), 1,3- and 1,4-bis(1-isocyanato-1-methylethyl)benzene (TMXDI), bis(4-(1-isocyanato-1-methylethyl)phenyl)carbonate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, toluene 2,4- and 2,6-diisocyanate and any mixtures of these isomers, diphenylmethane-2,4'- and / or -4,4'-diisocyanate and naphthalene-1,5-diisocyanate and any mixtures of such diisocyanates. Other equally suitable diisocyanates are also found, for example, in Justus Liebig's Annalen der Chemie, 562, 1949, 75-136.

[0044] Additionally or alternatively, OCN-Q-NCO is at least one uretdione polyisocyanate having two isocyanate groups.

[0045] Suitable uretdione units with two isocyanate groups are usually obtained by methods known in the art, optionally in the presence of a catalyst, by dimerizing monomeric diisocyanates described herein or their polyisocyanates. The example of an optional dimerization catalyst is: trialkylphosphine, aminophosphine and aminopyridine, such as dimethylaminopyridine and tris(dimethylamino)phosphine, and any other dimerization catalysts known to those skilled in the art. The result of the dimerization reaction depends on the catalyst used, process conditions and the diisocyanate adopted in a manner known to those skilled in the art. In particular, it is feasible for the product to be formed that it contains more than one uretdione group per molecule on average, and the number of uretdione groups is affected by distribution. The uretdione unit preferably contains 1-10 uretdione groups on average. Preferred uretdione units are prepared by the catalytic dimerization of PDI, HDI and / or IPDI.

[0046] In a preferred embodiment, the NCO-terminated prepolymers of the general formula (I) of the present invention are characterized in that Q is independently at least one aliphatic and / or cycloaliphatic group obtained by removing an isocyanate group from a diisocyanate, preferably selected from 1,5-diisocyanatopentane, 1,6-diisocyanatohexane, isophorone diisocyanate, 2,4′- and 4,4′-diisocyanatodicyclohexylmethane, 1,3- and 1,4-diisocyanatomethylcyclohexane, 1,3- and 1,4-xylylene diisocyanate and mixtures thereof, more preferably selected from 1,5-diisocyanatopentane, 1,6-diisocyanatohexane and / or isophorone diisocyanate.

[0047] Typically, the unit P in the NCO-terminated prepolymer of the general formula (I) of the present invention is at least one organic group obtained by removing hydroxyl groups from a polyol, which is preferably selected from polyether polyols, polyester polyols, polyurethane polyols, polysiloxane polyols, polycarbonate polyols, polybutadiene polyols, polyacrylate polyols, polymethacrylate polyols, copolymers of polyacrylate polyols and polymethacrylate polyols and mixtures thereof, more preferably selected from polyether polyols, polyester polyols, polyurethane polyols, polysiloxane polyols, polyacrylate polyols and mixtures thereof. In principle, these polyols are known to those skilled in the art.

[0048] Polyester polyol P(OH) p They are obtained in a manner known per se by reacting polyhydric alcohols, such as those mentioned above having 2 to 14 carbon atoms, with substoichiometric amounts of polycarboxylic acids, the corresponding carboxylic acid anhydrides, the corresponding polycarboxylic acid anhydride lower alcohols or lactones.

[0049] The acid or acid derivative used to prepare the polyester polyol can be aliphatic, alicyclic and / or aromatic and can be optionally substituted and / or unsaturated, for example substituted by halogen atoms. Examples of suitable acids are polycarboxylic acids or derivatives thereof with a molecular weight of 118 to 300 g / mol, such as succinic acid, adipic acid, sebacic acid, phthalic acid, isophthalic acid, trimellitic acid, phthalic anhydride, tetrahydrophthalic acid, maleic acid, maleic anhydride, dimerized and trimerized fatty acids, dimethyl terephthalate and diethylene glycol terephthalate.

[0050] Any desired mixtures of the starting compounds mentioned by way of example can also be used for the preparation of the polyester polyols.

[0051] One type of polyester polyols preferably used as polyol units P are those which can be prepared in a manner known per se from lactones and simple polyhydric alcohols, such as, for example, those mentioned above as starting molecules under ring opening. Examples of suitable lactones for preparing these polyester polyols are β-propiolactone, γ-butyrolactone, δ-valerolactone, ε-caprolactone, 3,5,5- and 3,3,5-trimethylcaprolactone or any mixtures of such lactones.

[0052] Suitable as polyol P(OH) p Polyhydroxy compounds of the polycarbonate type are in particular polycarbonate polyols known per se and which can be prepared, for example, by reacting dihydroxy alcohols (for example those mentioned in the above list of polyhydroxy alcohols having a molecular weight range of 62 g / mol to 400 g / mol) with diaryl carbonates (for example diphenyl carbonate), dialkyl carbonates (for example dimethyl carbonate) or phosgene.

[0053] Suitable as polyol P(OH) p Polyols of the polyester carbonate type are in particular diols which contain ester groups and carbonate groups and are known per se, as can be obtained, for example, according to the teaching of DE-A 1770245 or WO 03 / 002630 by reacting dihydric alcohols with, for example, lactones of the abovementioned type, in particular ε-caprolactone, and subsequently reacting the resulting polyester diols with diphenyl carbonate or dimethyl carbonate.

[0054] Suitable as polyol P(OH) pThe polyether polyols are in particular those having an average molecular weight (which can be calculated from the functionality and the hydroxyl number) of 800 g / mol to 3000 g / mol, preferably 900 g / mol to 2000 g / mol, more preferably 900 g / mol to 1500 g / mol, which are obtainable in a manner known per se by alkoxylation of suitable starter molecules. For the preparation of these polyether polyols, any desired polyhydric alcohols (such as the above-mentioned simple polyhydric alcohols having 2 to 14 carbon atoms) can be used as starter molecules. Alkoxylates suitable for the alkoxylation reaction are in particular ethylene oxide and propylene oxide, which can be used in any desired sequence and also in the form of mixtures for the alkoxylation reaction.

[0055] Suitable polyether polyols P(OH) p Also known per se are polyoxytetramethylene glycols which are formed by polymerization of tetrahydrofuran.

[0056] Suitable polyester polyols P(OH) p It can also be prepared by polycondensation of aliphatic dicarboxylic acids and / or their anhydrides with excess polyfunctional alcohols, and has a number average molecular weight of 800 g / mol to 3000 g / mol, preferably 900 g / mol to 2000 g / mol, more preferably 900 g / mol to 1500 g / mol, wherein the polyfunctional alcohol is a branched aliphatic diol, and its amount is at least 30% by weight, based on the total amount of the polyfunctional alcohol used.

[0057] Polyester polyols of this type are known. They are prepared in a manner known per se by methods such as those described in Gubbels, E. et al., 2018, Polyesters. In: Ullmann's Encyclopedia of Industrial Chemistry: Wiley-VCH Verlag GmbH & Co. KGaA, URL: https: / / doi.org / 10.1002 / 14356007.a21_227.pub2. If necessary, a catalytic amount of a standard esterification catalyst, such as an acid, a base or a transition metal compound, such as titanium tetrabutoxide, can be used. The esterification reaction is generally carried out in a temperature range of about 80°C to 260°C, preferably 100°C to 230°C, until the desired values ​​of hydroxyl number and acid number have been reached.

[0058] Starting compounds for the preparation of the polyester polyols are any desired straight-chain aliphatic or alicyclic, saturated or unsaturated dicarboxylic acids having 4 to 12 carbon atoms, preferably having 4 to 6 carbon atoms, or their anhydrides, and polyhydroxy aliphatic or alicyclic alcohols having 2 to 18 carbon atoms, preferably 2 to 6 carbon atoms, preferably diols and triols.

[0059] Suitable dicarboxylic acids or anhydrides for preparing the polyester polyols are, for example, succinic acid, succinic anhydride, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, itaconic anhydride, hexahydrophthalic acid, hexahydrophthalic anhydride, tetrahydrophthalic acid and tetrahydrophthalic anhydride, which can be used alone or in any desired mixtures with one another.

[0060] Suitable polyfunctional alcohols for preparing the polyester polyols are, for example, ethane-1,2-diol, propane-1,3-diol, butane-1,4-diol, pentane-1,5-diol, hexane-1,6-diol, heptane-1,7-diol, octane-1,8-diol, nonane-1,9-diol, decane-1,10-diol, dodecane-1,12-diol, cyclohexane-1,2-diol and cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, 4,4'-(1-methylethylidene)bicyclohexanol, propane-1,2,3-triol (glycerol), 1,1,1-trimethylolethane, hexane-1,2,6-triol, 1,1,1-trimethylolpropane, 2,2-bis(hydroxymethyl)propane

[0046] The invention also includes branched aliphatic diols, for example propane-1,2-diol, butane-1,3-diol, 2-methylpropanediol, 2,2-dimethyl-1,3-propanediol (neopentyl glycol), hexane-1,2-diol, 2-methylpentane-2,4-diol, 3-methylpentane-1,5-diol, 2-ethylhexane-1,3-diol, octane-1,2-diol, 2,2,4-trimethylpentane-1,5-diol, 2-butyl-2-ethylpropane-1,3-diol, 2,2,4- and / or 2,4,4-trimethylhexanediol, decane-1,2-diol or any desired mixtures of such alcohols. According to the invention, the polyfunctional alcohol is a branched aliphatic diol of the type described in an amount of at least 30% by weight, preferably at least 35% by weight, more preferably at least 40% by weight, based on the total amount of polyfunctional alcohol used.

[0061] Starter molecules for the ring-opening polymerization may be, for example, the difunctional alcohols or trifunctional alcohols mentioned above by way of example as suitable starter compounds for the preparation of further suitable polyester polyols or any desired mixtures of these alcohols.

[0062] The preparation of ε-caprolactone polyester polyols by ring-opening polymerization is generally carried out in the presence of a catalyst such as a Lewis acid or Bronsted acid, an organic tin or titanium compound at a temperature of 20 to 200°C, preferably 50 to 200°C.

[0063] Preferred polyester polyols are those which have been prepared using butane-1,4-diol, diethylene glycol, neopentyl glycol, hexane-1,6-diol, glycerol and / or 1,1,1-trimethylolpropane as starter molecules.

[0064] In a preferred embodiment, the NCO-terminated prepolymers of the general formula (I) according to the invention are characterized in that P in the general formula (I) is each independently at least one organic group obtained by removing hydroxyl groups from a polyol having an average molecular weight of ≥800 g / mol to ≤3000 g / mol and an OH functionality of >2 to ≤3, preferably an average molecular weight of ≥900 g / mol to ≤2000 g / mol and an OH functionality of >2 to ≤3, and more preferably an average molecular weight of ≥900 g / mol to ≤1500 g / mol and an OH functionality of >2 to ≤3. It is further preferred that P in the general formula (I) is each independently at least one polyol unit having an average molecular weight of ≥800 g / mol to ≤3000 g / mol and an OH functionality of >2 to <3, preferably an average molecular weight of ≥900 g / mol to ≤2000 g / mol and an OH functionality of >2 to <3, and more preferably an average molecular weight of ≥900 g / mol to ≤1500 g / mol and an OH functionality of >2 to <3.

[0065] It is even further preferred that P in the general formula (I) is at least one organic group obtained by removing hydroxyl groups from a polyester polyol having an average molecular weight of ≥800 g / mol to ≤3000 g / mol and an OH functionality of >2 to ≤3, preferably an average molecular weight of ≥900 g / mol to ≤2000 g / mol and an OH functionality of >2 to ≤3, and more preferably an average molecular weight of ≥900 g / mol to ≤1500 g / mol and an OH functionality of >2 to ≤3.

[0066] In a preferred embodiment, the inventive NCO-terminated prepolymers of the general formula (I) are characterized in that p is each independently a number of ≥2 to <4.5, preferably >2 to <3.

[0067] In principle, the NCO-terminated prepolymers according to the invention may contain or be diluted with solvents which are inert toward isocyanate groups, but this is not necessary. Suitable solvents are, for example, ethyl acetate, butyl acetate, ethylene glycol monomethyl ether or monoethyl ether acetate, 1-methoxyprop-2-yl acetate, 3-methoxy-n-butyl acetate, acetone, 2-butanone, 4-methyl-2-pentanone, cyclohexanone, toluene, xylene, chlorobenzene, white spirit, higher substituted aromatic compounds (for example known under the names Solventnapha, (Exxonmobil Chemical Central Europe, Cologne, Germany) and (commercially available aromatic compound species from Shell Deutschland Oil GmbH, Hamburg, Germany), and solvents such as propylene glycol diacetate, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, diethylene glycol ethyl and butyl ether acetate, N-methylpyrrolidone and N-methylcaprolactam, or any desired mixtures of such solvents.

[0068] The present invention further relates to a process for preparing the NCO-terminated prepolymer of the general formula (I) according to the present invention, the process comprising the following steps:

[0069] a) adding at least one polyol having a hydroxyl functionality of ≥2 to <3 and a polydispersity of ≥1.5 to a heated excess of at least one monomeric diisocyanate and / or at least one uretdione having two isocyanate groups in an NCO:OH group ratio of 4:1 to 20:1 to form urethane groups,

[0070] b) removing excess monomeric diisocyanate by distillation to an amount of <0.5 wt. %, preferably to <0.3 wt. %, and more preferably to <0.1 wt. %, based on the total solids content of the NCO-terminated prepolymer, to obtain the NCO-terminated prepolymer, and

[0071] c) optionally adding at least one solvent which is inert toward isocyanate groups.

[0072] The at least one polyol and the at least one monomeric diisocyanate and / or at least one uretdione having two isocyanate groups used in the process of the invention follow the same definitions and preferred embodiments outlined above in the description and claims of the NCO-terminated prepolymers of the invention, unless the context clearly indicates otherwise.

[0073] The polydispersity of the polyols to be used in the process of the invention can be measured in accordance with DIN 55672-1:2016-03.

[0074] At least one monomeric diisocyanate and / or at least one uretdione having two isocyanate groups is preferably reacted with at least one polyol at a temperature of 20 to 200°C, preferably 40 to 160°C, more preferably 60 to 140°C.

[0075] In a preferred embodiment of the process of the invention, the at least one polyol has an average molecular weight of ≥800 g / mol to ≤3000 g / mol, preferably ≥900 g / mol to ≤2000 g / mol and most preferably ≥900 g / mol to ≤1500 g / mol. This has the advantage that the content of oligomers with a number average molecular weight of ≤1000 g / mol in the NCO-terminated prepolymers of the invention can be further reduced to ≤17 wt.-%, more preferably ≥0.5 wt.-% to ≤17 wt.-%, even more preferably ≥1.0 wt.-% to ≤14 wt.-% and most preferably ≥1.5 wt.-% to ≤10 wt.-%, based on the total solids content of the NCO-terminated prepolymer.

[0076] In general, a polyol which already has this defined minimum average molecular weight can be used directly or, if a polyol having a lower average molecular weight should be used, it can be purified before the addition in step a), preferably in a distillation step, in order to increase the average molecular weight to the values ​​mentioned in the preceding paragraph.

[0077] Alternatively or additionally, it is preferred to carry out step b) of the process according to the invention at a temperature higher than that required for the removal of excess monomeric diisocyanate in order to further reduce the content of oligomers having a number average molecular weight of ≤1000 g / mol to ≤17 wt.-%, more preferably ≥0.5 wt.-% to ≤17 wt.-%, even more preferably ≥1.0 wt.-% to ≤14 wt.-%, and most preferably ≥1.5 wt.-% to ≤10 wt.-%, based on the total solids content of the NCO-terminated prepolymer. The aforementioned higher temperature depends on the type of monomers to be removed and can be determined by the skilled person by simple experiments without undue burden, for example by taking the thin film evaporation temperature of the monomeric diisocyanate to be removed and increasing this temperature by at least 10° C. but not more than 200° C.

[0078] The process according to the invention can be carried out without catalysis. However, if desired, suitable catalysts can also be used to accelerate the urethanization reaction. These are the customary catalysts known from polyurethane chemistry, for example tertiary amines, for example triethylamine, tributylamine, dimethylbenzylamine, diethylbenzylamine, pyridine, picoline, dicyclohexylmethylamine, dimethylcyclohexylamine, N,N,N′,N′-tetramethyldiaminodiethyl ether, bis(dimethylaminopropyl)urea, N-methyl- / N-ethylmorpholine, N-cocomorpholine, N-cyclohexylmorpholine, N,N,N′,N′-tetramethylethylenediamine, N,N,N′,N′-tetramethyl-1,3-butanediamine, N,N,N′,N′-tetramethyl-1,6-hexanediamine, diamines, pentamethyldiethylenetriamine, N-methylpiperidine, N-dimethylaminoethylpiperidine, N,N'-dimethylpiperazine, N-methyl-N'-dimethylaminopiperazine, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,2-dimethylimidazole, 2-methylimidazole, N,N-dimethylimidazole-β-phenylethylamine, 1,4-diazabicyclo[2.2.2]octane, bis(N,N-dimethylaminoethyl)adipate; alkanolamine compounds such as triethanolamine, triisopropanolamine, N-methyl and N-ethyldiamine; ethanolamine, dimethylaminoethanol, 2-(N,N-dimethylaminoethoxy)ethanol, N,N',N"-tris(dialkylaminoalkyl)hexahydrotriazines, for example N,N',N"-tris(dimethylaminopropyl)-s-hexahydrotriazine and / or bis(dimethylaminoethyl)ether; metal salts, for example inorganic and / or organic compounds of iron, lead, bismuth, zinc and / or tin in the conventional oxidation state of the metal, for example iron(II) chloride, iron(III) chloride, bismuth(III) 2-ethylhexanoate, bismuth(III) octanoate, bismuth(III) neodecanoate The invention also includes the following: lead octoate, zinc chloride, zinc 2-ethylhexanoate, tin(II) octoate, tin(II) ethylhexanoate, tin(II) palmitate, dibutyltin(IV) dilaurate (DBTL), dibutyltin(IV) dichloride or lead octoate; amidines, for example 2,3-dimethyl-3,4,5,6-tetrahydropyrimidine; tetraalkylammonium hydroxides, for example tetramethylammonium hydroxide; alkali metal hydroxides, for example sodium hydroxide, and alkali metal alkoxides, for example sodium methoxide and potassium isopropoxide, and alkali metal salts of long-chain fatty acids having 10 to 20 carbon atoms and optionally side OH groups.

[0079] These catalysts, if any, are preferably used in the process of the present invention in an amount of 0.001 to 5 wt %, more preferably 0.005 to 1 wt %, based on the total weight of all co-reactants, and they can be added before the start of the reaction or at any time during the reaction.

[0080] The progress of the reaction in the process according to the invention can be monitored by titrating the NCO content, for example in accordance with DIN EN ISO 11909:2007-05. When the desired NCO content has been reached, preferably when the NCO content which theoretically corresponds to complete conversion of isocyanate and hydroxyl groups has been reached in the reaction mixture, any urethanization catalyst used is preferably deactivated by adding a suitable catalyst poison.

[0081] Such catalyst poisons are, for example, inorganic acids, such as hydrochloric acid, phosphorous acid or phosphoric acid, acid chlorides, such as acetyl chloride, benzoyl chloride or isophthaloyl chloride, sulfonic acids and sulfonic esters, such as methanesulfonic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, perfluorobutanesulfonic acid, dodecylbenzenesulfonic acid, methyl p-toluenesulfonate and ethyl p-toluenesulfonate, mono- and dialkylphosphates, such as monotridecyl phosphate, dibutyl phosphate and dioctyl phosphate, and also silylated acids, such as trimethylsilylmethanesulfonate, trimethylsilyl trifluoromethanesulfonate, tris(trimethylsilyl)phosphate and diethyltrimethylsilylphosphate.

[0082] The amount of catalyst poison required to deactivate the catalyst is guided by the amount of catalyst used. Typically, an equivalent amount of catalyst poison is used based on the urethanization catalyst used initially. However, if any catalyst loss that occurs during the reaction is taken into account, even 20 to 80 equivalent % of catalyst poison based on the amount of catalyst originally used may be sufficient to stop the reaction.

[0083] The process of the invention is preferably carried out in the absence of solvent. However, if desired, suitable solvents which are inert to the reactive groups of the starting components may also be used. Suitable solvents are, for example, conventional coating solvents known per se, such as ethyl acetate, butyl acetate, ethylene glycol monomethyl ether or monoethyl ether acetate, 1-methoxyprop-2-yl acetate, 3-methoxy-n-butyl acetate, acetone, 2-butanone, 4-methyl-2-pentanone, cyclohexanone, toluene, xylene, chlorobenzene, white spirit, higher substituted aromatic compounds (for example known under the names Solventnaphtha, (ExxonMobil Chemical Central Europe, Cologne, Germany) and (commercially available aromatic compound species from Shell Deutschland Oil GmbH, Hamburg, Germany), and solvents such as propylene glycol diacetate, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, diethylene glycol ethyl and butyl ether acetate, N-methylpyrrolidone and N-methylcaprolactam, or any desired mixtures of such solvents.

[0084] Independently of the optional use of a solvent in step a) or b), the process of the invention comprises an optional step c) of adding at least one solvent inert toward isocyanate groups to achieve a preferred viscosity of <2000 mPas at 23° C. measured according to DIN EN ISO 3219:1994-10. Such optional solvents are preferably selected from the aforementioned list. If step c) is carried out, suitable solvents are preferably added in an amount to achieve a solids content of >50% by weight, more preferably a solids content of >80% by weight and most preferably a solids content of >95% by weight.

[0085] The present invention further relates to an NCO-terminated prepolymer for coating applications, preferably for manual coating applications, having the general formula (I),

[0086]

[0087] where P, Q and p are defined as follows

[0088] P is each independently at least one organic group obtained by removing a hydroxyl group from a polyol unit,

[0089] Q is each independently at least one organic group obtained by removing an isocyanate group from a monomeric diisocyanate unit and / or at least one organic group obtained by removing an isocyanate group from a uretdione unit having two isocyanate groups and

[0090] p is each independently a number ≥ 2.0, and

[0091] The NCO-terminated prepolymer has

[0092] a NCO content of ≥6.5 wt. % to ≤12.0 wt. %, based on the total solids content of the NCO-terminated prepolymer, and

[0093] a content of ≤17 wt. % of oligomers having a number average molecular weight ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, and

[0094] a monomeric diisocyanate content of <0.5% by weight, based on the total solids content of the NCO-terminated prepolymer, and

[0095] A mixture in which P does not contain the following substances

[0096] at least one polyester polyol unit A) having an average functionality of 1.9 to 2.3 and a number-average molecular weight of 300 to 3000 g / mol, which is prepared from aliphatic dicarboxylic acids and / or their anhydrides and an excess of polyfunctional alcohols, wherein the polyfunctional alcohols are branched aliphatic diols in an amount of at least 30% by weight, based on the total amount of polyfunctional alcohols, and

[0097] at least one polycaprolactone polyester unit B) having an average functionality of 2.0 to 3.0 and a number average molecular weight of 176 g / mol to 2000 g / mol,

[0098] In the NCO-terminated prepolymer, the polyester units A) account for 15% to 70% by weight of the total amount of the polyester units A) and B).

[0099] For this aspect, it is further preferred that P does not comprise polycaprolactone polyester units having an average functionality of 2.0 to 3.0 and a number average molecular weight of 176 to 2000 g / mol.

[0100] All embodiments and preferred embodiments disclosed herein for other aspects of the present invention can be combined with the two aforementioned aspects, except that suitable polyols P(OH) p Apart from the selection from the disclosed components in such a way that no mixture of polyester units A) and B) is claimed, and apart from the polydispersity of the NCO-terminated prepolymers of the invention can be below 2.0, but is preferably ≥ 2.0.

[0101] Therefore, the present invention further relates to a process for preparing the NCO-terminated prepolymer of the general formula (I) according to the present invention, which comprises the following steps:

[0102] a) adding at least one polyol having a hydroxyl functionality of ≥2 to <3 to a heated excess of at least one monomeric diisocyanate and / or at least one uretdione having two isocyanate groups in a ratio of NCO:OH groups of 4:1 to 20:1 to form urethane groups,

[0103] b) removing excess monomeric diisocyanate by distillation to an amount of <0.5 wt. %, preferably to <0.3 wt. %, and more preferably to <0.1 wt. %, based on the total solids content of the NCO-terminated prepolymer, to obtain an NCO-terminated prepolymer, and

[0104] c) optionally adding at least one solvent,

[0105] wherein the at least one polyol does not comprise a mixture of

[0106] at least one polyester polyol unit A) having an average functionality of 1.9 to 2.3 and a number-average molecular weight of 300 to 3000 g / mol, which is prepared from aliphatic dicarboxylic acids and / or their anhydrides and an excess of polyfunctional alcohols, wherein the polyfunctional alcohols are branched aliphatic diols in an amount of at least 30% by weight, based on the total amount of polyfunctional alcohols, and

[0107] at least one polycaprolactone polyester unit B) having an average functionality of 2.0 to 3.0 and a number average molecular weight of 176 g / mol to 2000 g / mol,

[0108] In the NCO-terminated prepolymer, the polyester units A) account for 15% to 70% by weight of the total amount of the polyester units A) and B).

[0109] For this process it is further preferred that the at least one polyol comprises no polycaprolactone polyester units at all having an average functionality of 2.0 to 3.0 and a number average molecular weight of 176 to 2000 g / mol.

[0110] The at least one polyol and the at least one monomeric diisocyanate and / or at least one uretdione having two isocyanate groups used in the process of the present invention follow the same definitions and preferred embodiments outlined above in the description, aspects and claims of the NCO-terminated prepolymers of the present invention, unless the context clearly indicates otherwise.

[0111] Due to the special physicochemical properties of the NCO-terminated prepolymers of the invention, they are particularly suitable for use in curable compositions for coatings, adhesives and / or sealants, which is a further aspect of the invention.

[0112] The invention further relates to a two-component system comprising or consisting of a component A) comprising at least one NCO-terminated prepolymer according to the invention and a component B) comprising at least one compound comprising at least one Zerevitinoff-reactive group.

[0113] Suitable compounds containing at least one Zerev-active group are, for example, the customary polymer polyether polyols, polyester polyols, polycarbonate polyols and / or polyacrylate polyols known from polyurethane chemistry, which generally have a number-average molecular weight of 200 to 22 000, preferably 250 to 18 000, particularly preferably 250 to 12 000. A comprehensive overview of suitable polymer polyols can be found, for example, in N. Adam et al., "Polyurethanes", Ullmann's Encyclopedia of Industrial Chemistry, electronic publication, 7th edition, Chapters 3.2-3.4, Wiley VCH, Weinheim 2005.

[0114] As an alternative to the above-mentioned hydroxy-functional compounds, polyamines, for example the polyaspartic acid derivatives known from EP-B 0 403 921, or those polyamines whose amino groups are present in blocked form (such as, for example, polyketimines, polyaldimines or oxazolidines) are also suitable as isocyanate-reactive adhesives. Under the influence of moisture, these blocked amino groups form free amino groups and, in the case of oxazolidines, also free hydroxyl groups which react crosslinkingly with isocyanate groups of polyisocyanates.

[0115] In a preferred embodiment, the at least one compound comprising at least one Zerev-reactive group is selected from polyester polyols, polyether polyols, polyurethane polyols, polyacrylate polyols, polymethacrylate polyols, polycarbonate polyols and mixtures thereof.

[0116] In another preferred embodiment, the component B) contains less than 5% by weight, preferably less than 2% by weight, more preferably less than 1% by weight of solvent. This has the advantage of further improving economy and work safety, since volatile organic emissions are significantly reduced without negatively affecting the properties of the two-component system of the invention. Suitable solvents can be selected from the customary solvents for such two-component systems and, for example, from the list described above for the NCO-terminated prepolymers of the invention and the process of the invention.

[0117] If appropriate, other auxiliaries and additives customary in the coating industry can be added to the spray system. Examples of suitable auxiliaries and additives are leveling agents, color pigments, filler materials, matting agents, inorganic or organic pigments, light stabilizers, paint additives (such as dispersants, leveling agents, thickeners, defoamers and other auxiliaries), adhesives, fungicides, biocides, stabilizers or inhibitors and catalysts or emulsifiers.

[0118] To control the curing speed, suitable catalysts can be used in the formulation of the coating composition, for example the urethanization catalysts customary in isocyanate chemistry, as described above, for example as catalysts for the preparation of the NCO-terminated prepolymers of the invention. If catalysts are used in the two-component system of the invention, they are preferably contained in compound B).

[0119] In all the uses described above for the NCO-terminated prepolymers according to the invention, they can be used alone or, for example, in admixture with any desired further polyisocyanates having aliphatically, cycloaliphatically, araliphatically and / or aromatically bonded isocyanate groups, more particularly with the known coating polyisocyanates having a uretdione, isocyanurate, iminooxadiazinedione, urethane, allophanate, biuret and / or oxadiazinetria structure, as described by way of example as isocyanate component in Laas et al., J. Prakt. Chem. 336, 1994, 185-200, DE-A 1670666, DE-A 3700209, DE-A 3900053, EP-A 0330966, EP-A 0366205, EP-A 0339396 and EP-A 0798299.

[0120] In the two-component systems of the invention for polyurethane and / or polyurea paints and coatings, which comprise the NCO-terminated prepolymers of the invention as crosslinker component or as a constituent of a crosslinker component for polyols, polythiols and / or polyamines, the co-reactant is generally present in such an amount that there are 0.5 to 3, preferably 0.6 to 2.0, more preferably 0.8 to 1.6 Zerewitinoff-active groups (also referred to herein as isocyanate-reactive groups) per isocyanate group.

[0121] The present invention further relates to a method for curing a composition on a substrate or in a cavity, the method comprising the following steps

[0122] i) applying at least one two-component system according to the invention to at least one substrate or in a cavity, and

[0123] ii) exposing the deposited composition to a temperature of 0°C to 120°C, preferably 20°C to 90°C, and more preferably 20°C to 60°C to cure the deposited cured composition.

[0124] Component A) and component B) of the two-component system are preferably mixed just before applying the two-component system to at least one substrate or into a cavity to obtain a mixture, which means that the mixture is preferably applied in step i). After the deposited composition cures, the cured composition forms a solid on the substrate or in the cavity. If the system is deposited on at least one substrate, such a solid is preferably a coating or an adhesive. If an adhesive, the second substrate is preferably added in a further step between steps i) and ii), or such a second substrate is added directly in step i). If the system is deposited in a cavity, such a solid is preferably a sealant or a foam.

[0125] Suitable substrates for coatings, adhesives and / or sealants formulated using the NCO-terminated prepolymers according to the invention or the two-component systems according to the invention include any desired substrates, for example metal, wood, glass, stone, ceramic materials, concrete, rigid and flexible plastics, textiles, leather and paper, which, before coating, may optionally also be provided with customary primers.

[0126] The present invention further relates to a cured article obtainable or obtained by the method of the present invention for curing a composition on a substrate or in a cavity. In a preferred embodiment, the cured composition is a repair coating and the substrate is a repair substrate. In this embodiment, the cured composition is preferably an automotive repair coating and the substrate is a repair automotive substrate. In another preferred embodiment, the cured composition is a foam or sealant in a building.

[0127] A further aspect of the invention is the use of the inventive NCO-terminated prepolymers or the inventive two-component systems for coatings, adhesives and / or sealants, in particular in automotive repair applications, or for foams and / or sealants, in particular in the construction industry.

[0128] The present invention particularly relates to the following embodiments:

[0129] According to a first aspect, the present invention relates to NCO-terminated prepolymers of the general formula (I) for use in coating applications,

[0130]

[0131] where P, Q and p are defined as follows

[0132] P is each independently at least one organic radical obtained by removing hydroxyl groups from polyol units having an average molecular weight of ≥800 g / mol to ≤3000 g / mol and an OH functionality of >2 to <3,

[0133] Q is each independently at least one aliphatic and / or alicyclic group obtained by removing an isocyanate group from a diisocyanate and

[0134] p is each independently a number ≥ 2.0, and

[0135] The NCO-terminated prepolymer has

[0136] a NCO content of ≥6.5 wt. % to ≤12.0 wt. %, based on the total solids content of the NCO-terminated prepolymer, and

[0137] a content of ≤17 wt. % of oligomers having a number average molecular weight ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, and

[0138] a <0.5 wt. % monomeric diisocyanate content, based on the total solids content of the NCO-terminated prepolymer and

[0139] Polydispersity a ≥ 2.0.

[0140] According to a second aspect, the present invention relates to an NCO-terminated prepolymer according to the first aspect, characterized in that the content of oligomers having a number average molecular weight of ≤1000 g / mol is ≥0.5% by weight to ≤17% by weight, preferably ≥1.0% by weight to ≤14% by weight, and most preferably ≥1.5% by weight to ≤10% by weight, based on the total solids content of the NCO-terminated prepolymer.

[0141] According to a third aspect, the present invention relates to an NCO-terminated prepolymer according to the first or second aspect, characterized in that the NCO-terminated prepolymer has an NCO content of ≥7.5% by weight to ≤11.0% by weight.

[0142] According to a fourth aspect, the present invention relates to an NCO-terminated prepolymer according to any one of the preceding aspects, characterized in that the NCO-terminated prepolymer has a number average molecular weight Mn of ≥1700 g / mol, preferably ≥1700 g / mol to ≤3500 g / mol, more preferably ≥1700 g / mol to ≤3100 g / mol.

[0143] According to a fifth aspect, the present invention relates to an NCO-terminated prepolymer according to any of the preceding aspects, characterized in that the NCO-terminated prepolymer has an average NCO functionality of >2.0, preferably >2.7.

[0144] According to a sixth aspect, the present invention relates to an NCO-terminated prepolymer according to any one of the preceding aspects, characterized in that Q in the general formula (I) is each independently at least one aliphatic and / or alicyclic group, which is obtained by removing the isocyanate group from a diisocyanate, wherein the diisocyanate is selected from 1,5-diisocyanatopentane, 1,6-diisocyanatohexane, isophorone diisocyanate, 2,4'- and 4,4'-diisocyanatodicyclohexylmethane, 1,3- and 1,4-diisocyanatomethylcyclohexane, 1,3- and 1,4-xylene diisocyanate and a mixture thereof, and is preferably selected from 1,5-diisocyanatopentane, 1,6-diisocyanatohexane and / or isophorone diisocyanate.

[0145] According to a seventh aspect, the present invention relates to an NCO-terminated prepolymer according to any one of the preceding aspects, characterized in that P in the general formula (I) is independently at least one polyol unit having an average molecular weight of ≥900 g / mol to ≤2000 g / mol and an OH functionality of >2 to <3, and more preferably an average molecular weight of ≥900 g / mol to ≤1500 g / mol and an OH functionality of >2 to <3.

[0146] According to an eighth aspect, the present invention relates to an NCO-terminated prepolymer according to any one of aspects one to six, characterized in that P in general formula (I) is independently at least one polyester polyol unit having an average molecular weight of ≥800 g / mol to ≤3000 g / mol and an OH functionality of >2 to <3, preferably an average molecular weight of ≥900 g / mol to ≤2000 g / mol and an OH functionality of >2 to <3, and more preferably an average molecular weight of ≥900 g / mol to ≤1500 g / mol and an OH functionality of >2 to <3.

[0147] According to a ninth aspect, the present invention relates to an NCO-terminated prepolymer according to any one of the preceding aspects, characterized in that p in the general formula (I) is each independently a number of ≥2 to <4.5, preferably >2 to <3.

[0148] According to a tenth aspect, the present invention relates to a method for preparing an NCO-terminated prepolymer according to any one of aspects one to nine, the method comprising the following steps:

[0149] a) adding at least one polyol having a hydroxyl functionality of ≥2 to <3 and a polydispersity of ≥1.5 to a heated excess of at least one monomeric diisocyanate in a ratio of NCO:OH groups of 4:1 to 20:1 to form urethane groups,

[0150] b) removing excess monomeric diisocyanate by distillation to an amount of <0.5 wt. %, preferably to <0.3 wt. %, and more preferably to <0.1 wt. %, based on the total solids content of the NCO-terminated prepolymer, to obtain the NCO-terminated prepolymer, and

[0151] c) optionally adding at least one solvent which is inert toward isocyanate groups.

[0152] According to an eleventh aspect, the present invention relates to a method according to the tenth aspect, characterized in that the at least one polyol has an average molecular weight of ≥800 g / mol to ≤3000 g / mol, preferably ≥900 g / mol to ≤2000 g / mol, and more preferably ≥900 g / mol to ≤1500 g / mol.

[0153] According to a twelfth aspect, the present invention relates to the use of the NCO-terminated prepolymer according to any one of aspects one to nine or the NCO-terminated prepolymer obtained by the method according to the tenth or eleventh aspect in a curable composition for coatings, adhesives and / or sealants.

[0154] According to a thirteenth aspect, the present invention relates to a two-component system comprising component A) and component B), wherein component A) comprises at least one NCO-terminated prepolymer according to any one of aspects 1 to 9, and component B) comprises at least one compound comprising at least one Zerevitenov-active group.

[0155] According to a fourteenth aspect, the present invention relates to a two-component system according to aspect thirteen, characterized in that component B) contains less than 5 wt. %, preferably less than 2 wt. %, more preferably less than 1 wt. % of organic solvent.

[0156] According to a fifteenth aspect, the present invention relates to a method for curing a composition on a substrate, the method comprising the following steps:

[0157] i) applying at least one two-component system according to aspect thirteen or fourteen to at least one substrate; and

[0158] ii) exposing the deposited composition to a temperature of 0°C to 120°C, preferably 20°C to 90°C, and more preferably 20°C to 60°C, to cure the deposited cured composition.

[0159] According to a sixteenth aspect, the present invention relates to a cured article obtainable or obtained, preferably directly obtained, by the method according to aspect fifteen.

[0160] The present invention is illustrated by reference to examples, although these examples should not be construed as limitative. Example:

[0161] All percentages are by weight unless otherwise indicated.

[0162] The NCO content is determined by titration in accordance with DIN EN ISO 11909:2007-05.

[0163] The residual monomer content is measured in accordance with DIN EN ISO 10283:2007-11 by gas chromatography with internal standard.

[0164] All viscosity measurements were performed according to DIN EN ISO 3219:1994-10 using a Physica MCR 51 rheometer from Anton Paar Germany GmbH (Germany) at 250 s. -1carried out at a shear rate of .

[0165] The number average molecular weights reported for the starting polyols are each calculated from the OH number and the OH functionality.

[0166] The content of oligomers with a number average molecular weight of ≤1000 g / mol is given as the number average molecular weight Mn determined via gel permeation chromatography (GPC at 23 ° C) with tetrahydrofuran as solvent. The measurement is carried out as described in DIN 55672-1: 2016-03: "Gelpermeationschromatographie, Teil 1-Tetrahydrofuran als Elutionsmittel" (SECurity GPC-System from PSS Polymer Service, flow 1.0 ml / min; column: 2×PSSSDV linear M, 8×300 mm, 5 um; RID-detector). Calibration is carried out using polystyrene standard samples of known molecular weight. The calculation of the number average molecular weight is carried out by software. The baseline value and the evaluation threshold are determined according to the DIN 55672-1 referenced above.

[0167] The NCO functionality is calculated using the following formula:

[0168]

[0169] The polydispersity is determined according to DIN 55672-1:2016-03.

[0170] Polyols:

[0171] Polyester polyol 1:

[0172] 19.0 parts by weight of trimethylolpropane based on 1,3-butane-1,3-diol, 13.8 parts by weight of neopentyl glycol, 23.1 parts by weight of 1,3-butane-1,3-diol, and 56.3 parts by weight of isophthalic acid were weighed into a flask and gradually heated to 200° C. under standard pressure while stirring, during which about 12.2 parts by weight of water were distilled off. The water removal was completed after about 20 hours.

[0173] The polyester polyols obtained in this way have the following characteristic data:

[0174]

[0175] Polyester polyol 2:

[0176] 17.2 parts by weight of neopentyl glycol, 13.3 parts by weight of butane-1,4-diol, 17.5 parts by weight of hexane-1,6-diol, 4.4 parts by weight of 2,2,4-trimethylpentane-1,3-diol, 4.4 parts by weight of 2-butyl-2-ethylpropane-1,3-diol and 43.2 parts by weight of adipic acid were weighed into a flask and gradually heated to 200° C. at standard pressure while stirring in the presence of 25 ppm of tin(II) chloride as a catalyst, during which about 5 parts by weight of water were distilled off.

[0177] After the removal of water had ended, a vacuum (15 mbar) was gradually applied over the course of about 4 hours, and the reaction was complete under these conditions in about a further 15 hours.

[0178] The polyester polyols obtained in this way have the following characteristic data:

[0179]

[0180] Polyester polyol 3:

[0181] ε-Caprolactone polyester initiated with hexane-1,6-diol

[0182]

[0183] Desmophen 1110 BD:

[0184] Linear polypropylene ether polyol, Covestro Deutschland AG

[0185]

[0186] NCO terminated prepolymer:

[0187] Embodiment 1 (present invention)

[0188] 1640 g of hexamethylene diisocyanate (HDI) were heated to a temperature of 100 ° C under nitrogen. 382 g of polyester polyol 1 with a functionality of 2.7 and an Mn of 988 g / mol was preheated to 80 ° C and then added to the mixture via a dropping funnel over 2 hours. The mixture was stirred for another 2 hours until the NCO content indicated complete conversion. Subsequently, excess HDI was removed via thin film evaporation at a temperature of 115 ° C and a pressure of 0.06 mbar. The product obtained was a slightly yellow, transparent NCO-terminated prepolymer with the following analytical characteristics:

[0189] The content of oligomers having a number-average molecular weight of ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, was 17% by weight.

[0190]

[0191] The prepolymer was dissolved in 30% methoxypropyl acetate (MPA).

[0192] Embodiment 2 (present invention)

[0193] 750 g of polyester polyol 1 having a functionality of 2.7 and an Mn of 988 g / mol were purified by thin-film evaporation at 195° C. and a pressure of 0.07 mbar.

[0194] 1630 g of hexamethylene diisocyanate (HDI) were heated to a temperature of 100 ° C under nitrogen. 442 g of pre-distilled polyester polyol 1 (Mn of 1110 g / mol) were preheated to 80 ° C and then added to the mixture via a dropping funnel over 4 hours. The mixture was stirred for another 2 hours until the NCO content indicated complete conversion. Subsequently, excess HDI was removed via thin film evaporation at a temperature of 115 ° C and a pressure of 0.02 mbar. The product obtained is a slightly yellow, transparent NCO-terminated prepolymer with the following analytical characteristics:

[0195] The content of oligomers having a number-average molecular weight of ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, is 3% by weight.

[0196]

[0197] The prepolymer was dissolved in 35% methoxypropyl acetate (MPA).

[0198] Embodiment 3 (present invention)

[0199] 750 g of polyester polyol 1 having a functionality of 2.7 and an Mn of 988 g / mol were purified by thin-film evaporation at 195° C. and a pressure of 0.07 mbar.

[0200] 1580 g of isophorone diisocyanate (IPDI) was heated to a temperature of 100° C. under nitrogen. 390 g of pre-distilled polyester polyol 1 (Mn of 1110 g / mol) was pre-heated to 80° C. and then added to the mixture via a dropping funnel over 6 hours. The mixture was stirred for another hour until the NCO content indicated complete conversion. Subsequently, excess IPDI was removed via thin film evaporation at a temperature of 180° C. and a pressure of 0.02 mbar. The product obtained was a yellow, transparent NCO-terminated prepolymer with the following analytical characteristics:

[0201] The content of oligomers having a number-average molecular weight of ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, is 3% by weight.

[0202]

[0203] The prepolymer was dissolved in 35% ethyl acetate (EA).

[0204] Example 4 (Comparative)

[0205] 920 g of isophorone diisocyanate (IPDI) were heated to a temperature of 100° C. under nitrogen. 600 g of polyether polyol Desmophen 1110BD (Mn 1002 g / mol) were added to the mixture via a dropping funnel over 6 hours. The mixture was stirred until the NCO content indicated complete conversion. Subsequently, excess IPDI was removed via thin film evaporation at a temperature of 180° C. and a pressure of 0.02 mbar. The product obtained was a yellow, transparent NCO-terminated prepolymer with the following analytical characteristics:

[0206] The content of oligomers having a number-average molecular weight of ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, was 1.6% by weight.

[0207]

[0208] Example 5 (Comparative)

[0209] 300 g of hexamethylene diisocyanate (HDI) were heated to a temperature of 100° C. under nitrogen. 277 g of polyether polyol Desmophen 1110BD (Mn 1002 g / mol) were added to the mixture via a dropping funnel over 6 hours. The mixture was stirred until the NCO content indicated complete conversion. Subsequently, excess HDI was removed via thin film evaporation at a temperature of 115° C. and a pressure of 0.03 mbar. The product obtained was a colorless, transparent NCO-terminated prepolymer with the following analytical characteristics:

[0210] The content of oligomers having a number-average molecular weight of ≤1000 g / mol was 1.0% by weight, based on the total solids content of the NCO-terminated prepolymer.

[0211]

[0212] Example 6 (Comparative, according to WO2016 / 116376, Example 2)

[0213] 1260 g of hexamethylene diisocyanate (HDI) introduced under dry nitrogen were stirred at a temperature of 100° C., and 215 g of polyester polyol 2 were added over the course of 90 minutes. After the addition had ended, the reaction mixture was stirred further at 110° C. until, after about 3 hours, an NCO content of 39.8% had been reached, corresponding to complete urethanization.

[0214] Unconverted monomeric HDI was removed on a thin-film evaporator at a temperature of 130° C. and a pressure of 0.1 mbar. This gave 382 g of a colorless, transparent prepolymer having the following characteristics:

[0215] The content of oligomers having a number-average molecular weight of ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, was 28.0% by weight.

[0216]

[0217]

[0218] Example 7 (Comparative, according to WO2016 / 116376, Example 3)

[0219] 1260 g of hexamethylene diisocyanate (HDI) were introduced with stirring under dry nitrogen at a temperature of 100° C., and 325 g of polyester polyol 3 were added over the course of 90 minutes. After the addition had ended, the reaction mixture was stirred further at 110° C. until, after about 3 hours, the NCO content had reached 37.1%, corresponding to complete urethanization.

[0220] Unconverted monomeric HDI was removed on a thin-film evaporator at a temperature of 130° C. and a pressure of 0.1 mbar. This gave 480 g of an initially colorless, transparent prepolymer which became cloudy and solidified after a few hours at room temperature. The semicrystalline product had the following characteristics:

[0221] The content of oligomers having a number-average molecular weight of ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, was 7.1% by weight.

[0222]

[0223] Application testing:

[0224] BYK 310 contains silicone surface additives, from BYK Chemie GmbH, Germany

[0225] Dibutyltin dilaurate (DBTL), 201, Lanxess Deutschland GmbH, Germany

[0226] DA 665BA acrylic polyol, OH content 4.6%, Allnex, Germany

[0227] 650MPA branched hydroxyl-containing polyester, OH content 5.3%, Covestro DeutschlandAG, Germany

[0228] 2488 branched polyester polyol, OH content 16%, Covestro Deutschland AG, Germany

[0229] DA 870 acrylic polyol, OH content 4.2%, Allnex, Germany

[0230] 1-Methoxypropyl-2-acetate (MPA), anhydrous, obtained from Azelis, Germany,

[0231] Toluene was obtained from Azelis, Germany.

[0232] Component A:

[0233] The polyols listed were combined with 0.1% Byk 310 and 0.03% catalyst DBTL and diluted with MPA.

[0234] Component B:

[0235] NCO terminated prepolymers of Examples 1-7.

[0236] Preparation : Components A and B were combined in a 1:1 ratio to produce a final solids content of 50%. The mixture was stirred by hand and then applied to the substrate. For glass plate applications, the formulation was applied using a coating knife. The dry coating thickness was about 50 μm. The coating was then cured at 60°C for 30 minutes. The coated glass plates were used for chemical testing and pendulum hardness experiments. Visual observations of the coatings were also recorded.

[0237] Pendulum hardness: According to The pendulum damping was determined on a glass plate in accordance with DIN EN ISO 1522:2007-04 and is given in Table 1 in seconds.

[0238] In order to test the solvent resistance of the coating, a small amount of the solvents xylene, 1-methoxypropyl-2-acetate, ethyl acetate and acetone are each placed in a test tube and a cotton wool pad is provided at the opening to form a solvent-saturated atmosphere in the test tube. The test tube is then placed on the surface of the coating on a glass plate together with the cotton pad, where they remain for 1 minute or 5 minutes. After the solvent has been wiped off, the film is checked for damage / softening / adhesion loss and rated (0: no change, 5: complete dissolution of the film). The 5 evaluations reported in Table 1 are evaluations of four solvents in the order of xylene (Xy), 1-methoxypropyl-2-acetate (MPA), ethyl acetate (EA) and acetone (Ac) in each case, expressed in the form of four consecutive numbers. These are determined according to DIN EN ISO 4628-1:2016-07.

[0239] Table 1: Overview of coating formulations and measured properties

[0240]

[0241]

[0242] *For these examples, the film was completely dissolved after 5 minutes, therefore the values ​​given were determined after 1 minute testing.

[0243] Discussion of the results in Table 1:

[0244] As can be seen from the results, the NCO-terminated prepolymers of the invention allow coatings to be obtained from formulations with commercial standard polyols. In contrast, the comparative formulations do not dry and result in viscous and soft coatings with insufficient hardness and limited solvent resistance.

Claims

1. An NCO-terminated prepolymer for coating applications having the general formula (I), where P, Q and p are defined as follows P is each independently at least one organic group obtained by removing a hydroxyl group from a polyol unit, Q is each independently at least one organic group obtained by removing an isocyanate group from a monomeric diisocyanate unit and / or at least one organic group obtained by removing an isocyanate group from a uretdione having two isocyanate groups and p is each independently a number ≥ 2.0, and The NCO-terminated prepolymer has a ≥6.5 wt. % to ≤12.0 wt. % NCO content, based on the total solids content of the NCO-terminated prepolymer, and a content of oligomers having a number average molecular weight of ≤1000 g / mol, based on the total solids content of the NCO-terminated prepolymer, of ≤17 wt. %, and a monomeric diisocyanate content of <0.5% by weight, based on the total solids content of the NCO-terminated prepolymer and Polydispersity a ≥ 2.

0.

2. The NCO-terminated prepolymer according to claim 1, It is characterized in that The content of oligomers with a number average molecular weight of ≤1000 g / mol is ≥0.5% to ≤17% by weight, preferably ≥1.0% to ≤14% by weight and most preferably ≥1.5% to ≤10% by weight, based on the total solids content of the NCO-terminated prepolymer.

3. The NCO-terminated prepolymer according to claim 1 or 2, It is characterized in that The NCO-terminated prepolymer has an NCO content of ≥7.5% by weight to ≤11% by weight.

4. The NCO-terminated prepolymer according to any one of claims 1 to 3, It is characterized in that The NCO-terminated prepolymer has a number average molecular weight Mn of ≥1700 g / mol, preferably ≥1700 g / mol to ≤3500 g / mol, more preferably ≥1700 g / mol to ≤3100 g / mol.

5. The NCO-terminated prepolymer according to any one of claims 1 to 4, It is characterized in that The NCO-terminated prepolymers have an average NCO functionality of >2.0, preferably >2.

7.

6. The NCO-terminated prepolymer according to any one of claims 1 to 5, It is characterized in that Q in the general formula (I) is each independently at least one aliphatic and / or alicyclic group obtained by removing an isocyanate group from a diisocyanate, preferably selected from 1,5-diisocyanatopentane, 1,6-diisocyanatohexane, isophorone diisocyanate, 2,4′- and 4,4′-diisocyanatodicyclohexylmethane, 1,3- and 1,4-diisocyanatomethylcyclohexane, 1,3- and 1,4-xylylene diisocyanate and mixtures thereof, more preferably selected from 1,5-diisocyanatopentane, 1,6-diisocyanatohexane and / or isophorone diisocyanate.

7. The NCO-terminated prepolymer according to any one of claims 1 to 6, It is characterized in that P in the general formula (I) is each independently at least one polyol unit having an average molecular weight of ≥800 g / mol to ≤3000 g / mol and an OH functionality of >2 to ≤3, preferably an average molecular weight of ≥900 g / mol to ≤2000 g / mol and an OH functionality of >2 to ≤3, and more preferably an average molecular weight of ≥900 g / mol to ≤1500 g / mol and an OH functionality of >2 to ≤3.

8. The NCO-terminated prepolymer according to any one of claims 1 to 7, It is characterized in that In the general formula (I), p is each independently a number of ≥2 to <4.5, preferably >2 to <3.

9. A method for preparing an NCO-terminated prepolymer according to any one of claims 1 to 8, the method comprising the following steps a) adding at least one polyol having a hydroxyl functionality of ≥2 to <3 and a polydispersity of ≥1.5 to a heated excess of at least one monomeric diisocyanate and / or at least one uretdione having two isocyanate groups in an NCO:OH group ratio of 4:1 to 20:1 to form urethane groups, b) removing excess monomeric diisocyanate by distillation to an amount of <0.5 wt. %, preferably to <0.3 wt. %, and more preferably to <0.1 wt. %, based on the total solids content of the NCO-terminated prepolymer, to obtain the NCO-terminated prepolymer, and c) optionally adding at least one solvent which is inert toward isocyanate groups.

10. The method according to claim 9, It is characterized in that The at least one polyol has an average molecular weight of ≧800 g / mol to ≦3000 g / mol, preferably ≧900 g / mol to ≦2000 g / mol, and more preferably ≧900 g / mol to ≦1500 g / mol.

11. Use of an NCO-terminated prepolymer according to any one of claims 1 to 8 or an NCO-terminated prepolymer obtained by the process according to claim 9 or 10 in a curable composition for coatings, adhesives and / or sealants. 12 . A two-component system comprising a component A) comprising at least one NCO-terminated prepolymer according to claim 1 and a component B) comprising at least one compound containing at least one Zerevitinoff-reactive group.

13. The two-component system according to claim 12, It is characterized in that The component B) comprises less than 5% by weight, preferably less than 2% by weight, more preferably less than 1% by weight of organic solvents.

14. A method for curing a composition on a substrate, said method comprising the following steps i) applying at least one two-component system according to claim 12 or 13 to at least one substrate; and ii) exposing the deposited composition to a temperature of 0°C to 120°C, preferably 20°C to 90°C, and more preferably 20°C to 60°C, to cure the deposited cured composition.

15. A cured article obtainable or obtained, preferably directly obtained, by the process according to claim 14.