Oxide semiconductor film, thin film transistor, and electronic device

By optimizing the crystal structure of the oxide semiconductor film, the field effect mobility of the thin film transistor is improved, the problem of low mobility in the existing technology is solved, and high mobility electrical properties and stable film properties are achieved.

CN118872074APending Publication Date: 2024-10-29JAPAN DISPLAY INC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380025339.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-02-20
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The field effect mobility of existing oxide semiconductor film thin film transistors is low, and it is hoped to improve the mobility by improving the crystal structure.

Method used

An oxide semiconductor film containing indium, gallium, yttrium, scandium and lanthanide elements is used, its crystal orientation is measured by the EBSD method, and the crystal structure is optimized to increase the occupancy of <111> and <101> to form a bixbyite-type structure A crystalline film that combines sputtering and annealing processes to control crystal grain size and orientation.

Benefits of technology

The field effect mobility of the thin film transistor is significantly improved, oxygen deficiency is suppressed, the insulating properties of the oxide semiconductor film are maintained, and high mobility electrical properties are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872074A_ABST
    Figure CN118872074A_ABST
Patent Text Reader

Abstract

The oxide semiconductor film is a crystalline oxide semiconductor film provided on the substrate, the oxide semiconductor film containing an indium (In) element and a first metal (M1) element selected from the group consisting of an aluminum (Al) element, a gallium (Ga) element, an yttrium (Y) element, a scandium (Sc) element, and a lanthanide element, and the oxide semiconductor film containing a plurality of crystal grains. Each of the plurality of crystal grains includes at least one of a crystal orientation < 001 >, a crystal orientation < 101 >, and a crystal orientation < 111 > obtained by an EBSD (Electron Back Scattering Diffraction) method. Among crystal orientation occupancy rates calculated on the basis of a measurement point having a crystal orientation in which the difference in crystal orientation with respect to the normal direction of the surface of the substrate is 0-15 DEG, the occupancy rate of crystal orientation < 111 > is greater than the occupancy rate of crystal orientation < 001 > and the occupancy rate of crystal orientation < 101 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to an oxide semiconductor film. Another embodiment of the present invention relates to a thin film transistor including the oxide semiconductor film. Another embodiment of the present invention relates to an electronic device including the thin film transistor. Background Art

[0002] In recent years, the development of thin film transistors using oxide semiconductor films as channels instead of silicon semiconductor films such as amorphous silicon, low-temperature polycrystalline silicon and single crystal silicon has been continuously developed (for example, see patent documents 1 to 6). Such thin film transistors including oxide semiconductor films can be formed with a simple structure and by a low-temperature process, just like thin film transistors including amorphous silicon films. In addition, it is known that thin film transistors including oxide semiconductor films have higher mobility than thin film transistors including amorphous silicon films.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2021-141338

[0006] Patent Document 2: Japanese Patent Application Publication No. 2014-099601

[0007] Patent Document 3: Japanese Patent Application Publication No. 2021-153196

[0008] Patent Document 4: Japanese Patent Application Publication No. 2018-006730

[0009] Patent Document 5: Japanese Patent Application Publication No. 2016-184771

[0010] Patent Document 6: Japanese Patent Application Publication No. 2021-108405 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, the field effect mobility of a thin film transistor including an existing oxide semiconductor film is not that high even when a crystalline oxide semiconductor film is used. Therefore, it is desired to improve the crystal structure of the oxide semiconductor film used in the thin film transistor to increase the field effect mobility of the thin film transistor.

[0013] One embodiment of the present invention is made in view of the above problems, and one of its purposes is to provide an oxide semiconductor film having a novel crystal structure. In addition, one of its purposes is to provide a thin film transistor including an oxide semiconductor film having a novel crystal structure. In addition, one embodiment of the present invention relates to an electronic device including a thin film transistor.

[0014] Means for solving problems

[0015] An oxide semiconductor film involved in one embodiment of the present invention is a crystalline oxide semiconductor film arranged on a substrate, the oxide semiconductor film contains an indium (In) element and a first metal (M1) element selected from the group consisting of an aluminum (Al) element, a gallium (Ga) element, an yttrium (Y) element, a scandium (Sc) element and a lanthanide element, the oxide semiconductor film contains a plurality of crystal grains, each of the plurality of crystal grains including at least one of a crystal orientation <001>, a crystal orientation <101> and a crystal orientation <111> obtained by an EBSD (electron backscatter diffraction) method, and in the occupancy of the crystal orientation calculated based on a measurement point having a crystal orientation difference of 0° to 15° with respect to a normal direction of a surface of the substrate, the occupancy of the crystal orientation <111> is greater than the occupancy of the crystal orientation <001> and the occupancy of the crystal orientation <101>.

[0016] A thin film transistor according to one embodiment of the present invention includes the above-mentioned oxide semiconductor film as a channel.

[0017] An electronic device according to one embodiment of the present invention includes the above-mentioned thin film transistor. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is an IPF mapping diagram of an oxide semiconductor film (Example) according to one embodiment of the present invention.

[0019] Figure 2 This is an IPF mapping diagram of an oxide semiconductor film (Example) according to one embodiment of the present invention.

[0020] Figure 3 This is a map showing the distribution of GOS in an oxide semiconductor film (Example) according to an embodiment of the present invention.

[0021] Figure 4 It is a cross-sectional view schematically showing a thin film transistor according to one embodiment of the present invention.

[0022] Figure 5 It is a plan view schematically showing a thin film transistor according to one embodiment of the present invention.

[0023] Figure 6This is a flowchart showing a method for manufacturing a thin film transistor according to one embodiment of the present invention.

[0024] Figure 7 It is a cross-sectional view showing a method for manufacturing a thin film transistor according to one embodiment of the present invention.

[0025] Figure 8 It is a cross-sectional view showing a method for manufacturing a thin film transistor according to one embodiment of the present invention.

[0026] Fig. 9 It is a cross-sectional view showing a method for manufacturing a thin film transistor according to one embodiment of the present invention.

[0027] Fig.10 It is a cross-sectional view showing a method for manufacturing a thin film transistor according to one embodiment of the present invention.

[0028] Fig.11 It is a cross-sectional view showing a method for manufacturing a thin film transistor according to one embodiment of the present invention.

[0029] Fig.12 It is a cross-sectional view showing a method for manufacturing a thin film transistor according to one embodiment of the present invention.

[0030] Fig.13 It is a cross-sectional view showing a method for manufacturing a thin film transistor according to one embodiment of the present invention.

[0031] Fig.14 This is a cross-sectional STEM image of a thin film transistor according to one embodiment of the present invention.

[0032] Fig.15 This is a cross-sectional STEM image of a thin film transistor according to one embodiment of the present invention.

[0033] Fig.16 It is a schematic diagram showing an electronic device according to one embodiment of the present invention.

[0034] Fig.17 This is an IPF mapping diagram of a conventional oxide semiconductor film (comparative example).

[0035] Fig.18 This is an IPF mapping diagram of a conventional oxide semiconductor film (comparative example).

[0036] Fig.19 It is a map showing the distribution of GOS of a conventional oxide semiconductor film (comparative example). DETAILED DESCRIPTION

[0037] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings. The following disclosure is only an example. The configuration that can be easily conceived by those skilled in the art by appropriately changing the configuration of the embodiment while maintaining the gist of the invention is of course included in the scope of the present invention. With respect to the accompanying drawings, in order to make the description clearer, the width, thickness, shape, etc. of each part are sometimes schematically indicated compared to the actual method. However, the shape shown in the figure is only an example and does not limit the interpretation of the present invention. In this specification and each figure, the same figure mark is marked for the same elements as those described in the accompanying drawings that have appeared, and the detailed description is sometimes appropriately omitted.

[0038] In this specification, the direction from the substrate toward the oxide semiconductor layer is referred to as up or above. Conversely, the direction from the oxide semiconductor layer toward the substrate is referred to as down or below. Thus, for ease of explanation, the phrases such as above or below are used for explanation, but, for example, the up-and-down relationship between the substrate and the oxide semiconductor layer may be configured in a manner opposite to that shown in the figure. In the following description, for example, the expression such as the oxide semiconductor layer on the substrate is only used to illustrate the up-and-down relationship between the substrate and the oxide semiconductor layer as described above, and other components may be configured between the substrate and the oxide semiconductor layer. Above or below means the stacking order in a structure having multiple layers stacked, and in the case of a pixel electrode described as above the transistor, it may also be a positional relationship in which the transistor and the pixel electrode do not overlap when viewed from above. On the other hand, in the case of a pixel electrode described as vertically above the transistor, it means a positional relationship in which the transistor and the pixel electrode overlap when viewed from above.

[0039] In the present specification, the term "film" and the term "layer" can be used interchangeably according to circumstances.

[0040] A “display device” refers to a structure that uses an electro-optical layer to display an image. For example, a term such as a display device sometimes refers to a display panel including an electro-optical layer, or sometimes refers to a structure that is equipped with other optical components (such as polarization components, backlight sources, touch panels, etc.) relative to a display unit. As long as there is no technical contradiction, the “electro-optical layer” may include a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer. Therefore, with respect to the embodiments described later, as display devices, a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer are exemplified for explanation, but the structure in this embodiment can be applied to a display device including the other electro-optical layers mentioned above.

[0041] In this specification, unless otherwise specified, expressions such as “α includes A, B, or C”, “α includes any one of A, B, and C”, and “α includes one selected from the group consisting of A, B, and C” do not exclude the case where α includes multiple combinations of A to C. In addition, the above expressions do not exclude the case where α includes other elements.

[0042] It should be noted that the following embodiments can be combined with each other as long as no technical contradiction occurs.

[0043] <First embodiment>

[0044] Reference Figure 1 to Figure 3 An oxide semiconductor film according to one embodiment of the present invention will be described.

[0045] [1. Composition of Oxide Semiconductor Film]

[0046] The oxide semiconductor film involved in this embodiment contains an indium (In) element and a first metal (M1) element selected from the group consisting of an aluminum (Al) element, a gallium (Ga) element, an yttrium (Y) element, a scandium (Sc) element and a lanthanide element. In the composition ratio of the oxide semiconductor film, the atomic ratio of the indium element to the metal element (M) other than the indium element preferably satisfies formula (1). In other words, the ratio of the indium element in the oxide semiconductor film is preferably greater than 50%. By increasing the ratio of the indium element, a crystalline oxide semiconductor film can be formed. In addition, the crystal structure of the oxide semiconductor film preferably has a pyroxene-type structure. By increasing the ratio of the indium element, an oxide semiconductor film having a pyroxene-type structure can be formed.

[0047] [Mathematical formula 1]

[0048]

[0049] The first metal element is preferably gallium. Since gallium and indium are both Group 13 elements, gallium does not hinder the crystallinity of the oxide semiconductor film. That is, even if the oxide semiconductor film contains gallium as the first metal element, an oxide semiconductor film having a pyrolusite structure can still be formed.

[0050] In the case where the first metal element is gallium, the oxide semiconductor film may also include a second metal (M2) element selected from the group consisting of aluminum, yttrium, scandium and lanthanide elements. In this case, in the composition ratio of the oxide semiconductor film, the atomic ratio of indium, gallium and the second metal element preferably satisfies formula (2), formula (3) and formula (4). Since the ratio of the second metal element is lower than that of the indium element or the gallium element, the second metal element does not hinder the crystallinity of the oxide semiconductor.

[0051] [Mathematical formula 2]

[0052]

[0053] [Mathematical formula 3]

[0054]

[0055] [Formula 4]

[0056]

[0057] The detailed manufacturing method of the oxide semiconductor film will be described later, and the oxide semiconductor film can be formed using a sputtering method. The composition of the oxide semiconductor film formed by sputtering depends on the composition of the sputtering target. In the sputtering target having the above composition, an oxide semiconductor film having no composition deviation of the metal element can be formed by sputtering. Therefore, the composition of the metal elements (for example, indium element, M1 element or M2 element, etc.) of the oxide semiconductor film can also be regarded as being equal to the composition of the metal elements of the sputtering target. For example, the composition of the metal elements of the oxide semiconductor film can be determined based on the composition of the metal elements of the sputtering target. It should be noted that since the oxygen element contained in the oxide semiconductor film will change according to the process conditions of the sputtering, etc., it is not limited to this.

[0058] In addition, the composition of the metal elements of the oxide semiconductor film can also be determined by fluorescent X-ray analysis or EPMA (Electron Probe Micro Analyzer) analysis, etc. In addition, since the oxide semiconductor film is crystalline, the composition of the metal elements of the oxide semiconductor film can also be determined based on the crystal structure and lattice constant using an XRD (X-ray Diffraction) method.

[0059] [2. Crystal structure of oxide semiconductor film]

[0060] The oxide semiconductor film according to this embodiment has crystallinity. The crystal structure of the oxide semiconductor film is not particularly limited, but is preferably a bixbyite structure. The crystal structure of the oxide semiconductor film can be determined using an XRD method or an electron beam diffraction method.

[0061] In addition, the oxide semiconductor film involved in this embodiment includes a plurality of crystal grains. The inventors of the present application have found that the crystal grains of the oxide semiconductor film involved in this embodiment have characteristics different from those of the crystal grains of the existing oxide semiconductor film. Specifically, the inventors of the present application have found an oxide semiconductor film having a new crystal structure including crystal grains different from the existing crystal grains. The oxide semiconductor film having such a new crystal structure can be measured using the electron backscatter diffraction (EBSD) method. Therefore, the measurement of the oxide semiconductor film based on the EBSD method is described below.

[0062] [2-1.EBSD method]

[0063] The EBSD method is an analysis method that irradiates an object to be measured with an electron beam, analyzes the electron backscatter diffraction generated on each crystal plane of the crystal structure of the object to be measured, and measures the crystal structure in the measurement area of ​​the object to be measured. The EBSD method analyzes the data obtained from an EBSD detector mounted on a scanning electron microscope (SEM) or a transmission electron microscope (TEM), thereby obtaining information such as the grain or crystal orientation of the oxide semiconductor film in the measurement area.

[0064] [2-2.IPF Mapping Diagram]

[0065] The IPF (Inverse Pole Figure) map is an image obtained by color-coding the crystal orientation according to a specified color key. In the measurement using the EBSD method, since the information of the crystal orientation can be obtained, an IPF map can be made based on the information of the crystal orientation obtained. In the IPF map, the areas of the regions separated by colors for multiple crystal orientations can also be obtained, and the ratio (hereinafter referred to as "occupancy") relative to the overall area of ​​the measurement area can be calculated for quantitative comparison.

[0066] The IPF map may also be an image obtained by extracting data from measurement points whose crystal orientation difference relative to the normal direction of the surface of the substrate (or the surface of the oxide semiconductor film) is within a specified range. For example, the specified range is above 0° and below 15°. In the IPF map obtained by extracting the data of a specific measurement point in this way, the measurement points having a crystal orientation that is greatly inclined from the normal direction of the surface of the substrate are excluded, so that the crystal orientation that is easy to orient among multiple crystal orientations can be made obvious. Therefore, in the IPF map obtained by extracting the data of a specific measurement point, the occupancy rates of each of the multiple crystal orientations are compared, and the crystal orientation that is easy to orient can be determined more clearly.

[0067] In the case where the oxide semiconductor film involved in the present embodiment has a bixbyite structure, within the range of a crystal orientation difference of 0° to 15° with respect to the normal direction of the surface of the substrate, the occupancy of the crystal orientation <111> is greater than the occupancy of the crystal orientation <001> and the occupancy of the crystal orientation <101>. In addition, the occupancy of the crystal orientation <101> is greater than the occupancy of the crystal orientation <001>. In particular, in the oxide semiconductor film involved in the present embodiment, the occupancy of the crystal orientation <001> is greatly reduced, which is a feature that has not been found in existing oxide semiconductor films. In the oxide semiconductor film involved in the present embodiment, the combined occupancy of the crystal orientation <101> and the crystal orientation <111> is more than 10 times the occupancy of the crystal orientation <001>. On the other hand, in existing oxide semiconductor films, the combined occupancy of the crystal orientation <101> and the crystal orientation <111> is less than 10 times the occupancy of the crystal orientation <001>. In the oxide semiconductor film according to this embodiment, the occupancy of the crystal orientation <101> is preferably 4.5 times or more than the occupancy of the crystal orientation <001>. The occupancy of the crystal orientation <111> is preferably 4 times or more than the occupancy of the crystal orientation <001>.

[0068] Here, the crystal orientation <001> represents

[001] and its equivalents

[100] and

[010] . In addition, the crystal orientation <101> represents

[101] and its equivalents

[110] and

[011] . In addition, the crystal orientation <111> represents

[111] . In addition, in each orientation, "1" can also be "-1", which is regarded as an axis equivalent to each orientation.

[0069] It should be noted that in crystal orientation, in addition to <001>, <101> and <111>, there are also <hk0> (h≠k, h and k are natural numbers), <hhl> (h≠l, h and l are natural numbers) and <hkl> (h≠k≠l, h, k and l are natural numbers).

[0070] [2-3. Grains]

[0071] A grain is a crystalline region surrounded by a grain boundary. In the EBSD method, since information related to the crystal orientation can be obtained, the grain boundary can be defined based on the crystal orientation. Generally, when the crystal orientation difference between two adjacent measurement points exceeds 5°, it is defined as the grain boundary between them. Therefore, in the oxide semiconductor film involved in this embodiment, the above definition is also applicable.

[0072] [2-4. Crystalline particle size]

[0073] The crystal grain size is a value indicating the size of a crystal grain. In the EBSD method, the area S of the crystal grain can be calculated, and therefore the diameter of a circle corresponding to the area S is defined as the crystal grain size d.

[0074] [2-5. Average crystal particle size]

[0075] The average crystal grain size is the average value of the crystal grain sizes of a plurality of crystal grains. Since the oxide semiconductor film according to this embodiment includes a plurality of crystal grains, the average crystal grain size can be used to evaluate the oxide semiconductor film. AVE Calculate using formula (5). Here, A j is the area ratio of the jth grain (the ratio of the area of ​​the grain to the area of ​​the entire EBSD measurement area (measurement area)), d j is the crystal grain size of the jth grain, and N is the number of grains. As shown in formula (5), the average crystal grain size d AVE is the average area value in the measurement area weighted by the area of ​​the grains. AVE If the value is large, it can be said that a large number of crystal grains having a large crystal grain size exist in the oxide semiconductor film.

[0076] [Mathematical formula 5]

[0077]

[0078] The average crystal grain size of the plurality of crystal grains included in the oxide semiconductor film according to this embodiment is, for example, 0.1 μm or more, preferably 0.3 μm or more, and more preferably 0.5 μm or more.

[0079] [2-6. Maximum crystal particle size]

[0080] The maximum crystal grain size is the maximum value of the crystal grain sizes of the plurality of crystal grains. The maximum crystal grain size of the crystal grains included in the oxide semiconductor film according to this embodiment is, for example, 0.5 μm or more, preferably 0.8 μm or more, and more preferably 1.0 μm or more.

[0081] [2-7.GOS]

[0082] GOS (Grain Orientation Spread) is a value indicating the crystal orientation difference within a grain. GOS is calculated using formula (6). That is, GOS is the crystal orientation θ of the i-th measurement point within the grain. i The average crystal orientation θ of n measurement points in the grain AVE The value obtained by dividing the difference of by n measurement points in the grain. In other words, GOS is the value obtained by averaging the crystal orientation in the grain. GOS represents the magnitude of the strain in the grain. It can be said that the larger the GOS, the larger the strain in the grain.

[0083] [Mathematical formula 6]

[0084]

[0085] [2-8.GOS average value]

[0086] The average GOS value is the average value of the GOS values ​​of a plurality of crystal grains. Since the oxide semiconductor film according to this embodiment includes a plurality of crystal grains, the average GOS value can be used to evaluate the oxide semiconductor film. AVE Calculate using formula (7). Here, A j is the area ratio of the jth grain, GOS j is the GOS of the jth grain, and N is the number of grains. As shown in formula (7), the average GOS GOS AVE It is the average value of the area in the measurement area weighted by the area of ​​the grain. AVE If the value is large, it can be said that a large number of crystal grains whose crystal orientations are greatly changed exist in the oxide semiconductor film.

[0087] [Mathematical formula 7]

[0088]

[0089] As described above, the oxide semiconductor film involved in this embodiment includes grains whose crystal orientation changes greatly, and the number of such grains is reflected as the GOS average value. In the oxide semiconductor film involved in this embodiment, the GOS average value is greater than 2°. The GOS average value of the existing oxide semiconductor film is less than 1°, and the large GOS average value is also one of the characteristics of the oxide semiconductor film involved in this embodiment.

[0090] In the existing oxide semiconductor film, if the crystal orientation within the grains changes significantly, the strain of the grains increases, which will hinder the crystal growth of the grains, so that large grains cannot be formed. However, in the oxide semiconductor film involved in the present embodiment, although the change in the crystal orientation within the grains is large, the grains contained in the oxide semiconductor film involved in the present embodiment have an average crystal grain size or maximum crystal grain size that is equal to or greater than that of the existing oxide semiconductor. In addition, usually if the change in the crystal orientation within the grains is large, lattice defects are easily generated, resulting in a decrease in the insulating properties (or semiconductor properties) of the oxide semiconductor film. However, in the oxide semiconductor film involved in the present embodiment, crystal nuclei with a specific crystal orientation are generated by optimizing the sputtering film forming conditions, thereby suppressing the amount of oxygen deficiencies in the film after heat treatment, and the insulating properties will not be reduced. For example, a thin film transistor using the oxide semiconductor film as a channel has excellent electrical properties with high mobility.

[0091] It should be noted that the measurement of the crystal structure of the oxide semiconductor film according to the present embodiment is not limited to the EBSD method, and other measurement methods other than the EBSD method may be used to measure the crystal orientation or the change in the crystal orientation within the crystal grain.

[0092] [3. Method for producing oxide semiconductor film]

[0093] The oxide semiconductor film according to this embodiment is produced by a sputtering process and an annealing process.

[0094] In the sputtering process, an oxide semiconductor film is formed on a substrate. The oxide semiconductor film after the sputtering process is preferably a film with less crystalline components, and is particularly preferably amorphous. In the film formation based on sputtering, since the ions generated in the plasma and the atoms knocked back by the sputtering target collide with the substrate, even if the substrate temperature is room temperature at the start of sputtering, the substrate temperature will rise during the film formation. If the substrate temperature rises during the film formation, the oxide semiconductor film just after the film formation will contain microcrystals, and grains with a crystal orientation of <001> are easily generated through the subsequent annealing process. Therefore, it is preferred to form the oxide semiconductor film while controlling the substrate temperature. The substrate temperature is, for example, below 100°C, preferably below 70°C, and more preferably below 50°C. The substrate temperature can also be below 30°C. The substrate temperature can be controlled, for example, by cooling the substrate. In addition, the oxide semiconductor film can also be formed at a film formation rate at which the substrate temperature does not exceed a specified temperature. In addition, the distance between the target and the substrate can be increased to control the substrate temperature by adjusting the substrate in a manner that is not affected by the sputtering target.

[0095] As the substrate for forming the oxide semiconductor film, a rigid substrate such as a glass substrate, a quartz substrate, or a sapphire substrate, or a flexible substrate such as a polyimide substrate, an acrylic substrate, a siloxane-based substrate, or a fluororesin substrate can be used. In addition, the substrate for forming the oxide semiconductor film can also be a substrate formed with silicon oxide (SiO x ) film, silicon oxynitride (SiO x N y ) film, silicon nitride (SiN x ) film, silicon oxynitride (SiN x O y ) film, aluminum oxide (AlO x ) film, aluminum oxynitride (AlO x N y ), aluminum oxynitride (AlN x O y ) or aluminum nitride (AlN x ) substrate.

[0096] In the annealing process, the oxide semiconductor film is crystallized. The annealing is maintained at a predetermined reaching temperature for a predetermined time. The predetermined reaching temperature is 300° C. to 500° C., preferably 350° C. to 450° C. In addition, the holding time at the reaching temperature is 15 minutes to 120 minutes, preferably 30 minutes to 60 minutes.

[0097] [4. Example]

[0098] The oxide semiconductor film according to this embodiment is described in more detail based on specific examples. It should be noted that the example described below is one example of the oxide semiconductor film according to this embodiment, and the structure of the oxide semiconductor according to this embodiment is not limited to the structure of the example described below.

[0099] [4-1. Production method]

[0100] (Example)

[0101] As an example, the oxide semiconductor film involved in this embodiment is produced on a substrate using the above-mentioned sputtering process and annealing process. In the sputtering process, a sputtering target containing indium (In) element and gallium (Ga) element as the first metal (M1) element in the sintered body and the indium element is 70% or more in atomic ratio relative to all the metal elements contained in the sintered body is used to form an oxide semiconductor film on a glass substrate. The oxygen partial pressure during film formation is 10.0 (%), and the substrate temperature is controlled in a manner such that the substrate temperature during film formation is below 100°C. Afterwards, the oxide semiconductor film is subjected to an annealing process in an atmospheric atmosphere. In the annealing process, the control is performed in a manner such that the reaching temperature becomes 450°C, and the reaching temperature is maintained for 60 minutes. The chemical composition of the oxide semiconductor film is the same as that of the sputtering target. It should be noted that the first metal (M1) element contained in the sintered body of the embodiment is not limited to gallium (Ga) element, and even aluminum (Al) element, yttrium (Y) element, scandium (Sc) element and lanthanide element will have the same effect.

[0102] (Comparative Example)

[0103] As a comparative example, an existing oxide semiconductor film is produced on a substrate using an existing sputtering process and an annealing process. In the sputtering process, a sputtering target is used in which an indium (In) element and a gallium (Ga) element as a first metal (M1) element are contained in a sintered body, and the indium element is more than 70% in atomic ratio relative to all metal elements contained in the sintered body, and an oxide semiconductor film is formed on a quartz substrate. The oxygen partial pressure during film formation is 10.0 (%), and the substrate temperature is not controlled during film formation. Afterwards, the oxide semiconductor film is subjected to an annealing process in an atmospheric atmosphere. In the annealing process, the reaching temperature is controlled to be 450°C, and the reaching temperature is maintained for 60 minutes. The chemical composition of the oxide semiconductor film is the same as that of the sputtering target. It should be noted that the first metal (M1) element contained in the sintered body of the embodiment is not limited to the gallium (Ga) element, and even aluminum (Al) elements, yttrium (Y) elements, scandium (Sc) elements and lanthanide elements will have the same effect.

[0104] The fabrication conditions (film formation conditions and annealing conditions) of the examples and comparative examples are shown in Table 1. Although the film thickness of the oxide semiconductor film is different between the examples and comparative examples, the major difference lies in whether the substrate temperature is controlled during film formation.

[0105] [Table 1]

[0106]

[0107] [4-2. Crystal structure analysis by XRD method]

[0108] The crystal structures of the oxide semiconductor film of the example and the oxide semiconductor film of the comparative example were analyzed using the XRD method. The oxide semiconductor film of the example and the oxide semiconductor film of the comparative example were both crystalline and had a bixbyite-type crystal structure.

[0109] [4-3. Crystal orientation analysis using the EBSD method]

[0110] The crystal orientation analysis of the oxide semiconductor film of the embodiment and the oxide semiconductor film of the comparative example was performed using the EBSD method. The measurement conditions of the EBSD method are shown in Table 2. In addition, the analysis of the crystal orientation used OIM-Analysis (version 7.1) manufactured by TSL Solutions. The crystal structure was located using the crystal structure file of 14388 of the bixbyite structure of ICSD (Inorganic Crystal Structure Database: Chemical Information Association). The results of the measurement and analysis judged that the pattern obtained when the CI value became 0.6 or more was clear enough, and the crystal orientation was identified as a bixbyite structure.

[0111] [Table 2]

[0112]

[0113] The IPF mapping diagram of the oxide semiconductor film of the embodiment is as follows: Figure 1 and Figure 2 In addition, the IPF mapping diagram of the oxide semiconductor film of the comparative example is shown in Fig.17 and Fig.18 As shown. Figure 1 , Figure 2 , Fig.17 and Fig.18 In FIG. 1 , the black lines indicate grain boundaries. That is, in both the oxide semiconductor film of the example and the oxide semiconductor thin film of the comparative example, a plurality of crystal grains surrounded by the black lines can be confirmed. Figure 1 , Figure 2 , Fig.17 and Fig.18 The IPF maps shown are color-coded according to the color keys shown in the respective figures. In particular, the colors are coded in such a way that the crystal orientation <001> is colored red, the crystal orientation <101> is colored green, and the crystal orientation <111> is colored blue. Figure 2 and Fig.18 In the method, the color differentiation is performed by extracting the measurement points where the crystal orientation difference of the crystal orientation <001>, crystal orientation <101> or crystal orientation <111> relative to the normal direction of the substrate surface (or the surface of the oxide semiconductor film) is within the range of 0° to 15°. In other words, Figure 2 and Fig.18 They are Figure 1 and Fig.17 The image is obtained by excluding the measurement points where the crystal orientation difference of the crystal orientation <001>, the crystal orientation <101> or the crystal orientation <111> exceeds 15° with respect to the normal direction of the surface of the substrate.

[0114] The average crystal grain size of the oxide semiconductor film of the example was calculated to be 0.61 (μm). On the other hand, the average crystal grain size of the oxide semiconductor film of the comparative example was calculated to be 0.65 (μm).

[0115] The maximum crystal grain size of the oxide semiconductor film of the example was 1.1 (μm). On the other hand, the maximum crystal grain size of the oxide semiconductor film of the comparative example was also 1.1 (μm).

[0116] If Figure 2 The IPF map shown is similar to Fig.18 Compared with the IPF map shown in Figure 2 In the IPF map shown, many areas are divided by blue. Fig.18 In the IPF map shown, many areas are distinguished by green color. Figure 2 (i.e., the measurement points of the crystal orientation having a crystal orientation difference of 0° to 15° with respect to the normal direction of the surface of the substrate) were used to calculate the occupancy rates of the crystal orientation <001>, crystal orientation <101>, and crystal orientation <111> of the oxide semiconductor film of the embodiment within the measurement area, and the results were 1.8(%), 14.7(%), and 39.2(%), respectively. Fig.18 (that is, a measurement point of a crystal orientation having a crystal orientation difference of more than 0° and less than 15° with respect to the normal direction of the surface of the substrate), the occupancy rates of the crystal orientation <001>, crystal orientation <101> and crystal orientation <111> of the oxide semiconductor film of the comparison example in the measurement area were calculated, and the results were 5.6(%), 23.3(%) and 19.8(%), respectively.

[0117] In the oxide semiconductor film of the embodiment, the occupancy of the crystal orientation <001> is lower than the occupancy of the crystal orientation <101> and the crystal orientation <111>. In other words, the occupancy of the crystal orientation <101> and the crystal orientation <111> is higher than the occupancy of the crystal orientation <001>. In the oxide semiconductor film of the embodiment, the occupancy of the crystal orientation <101> and the occupancy of the crystal orientation <111> are 8.2 times and 21.8 times the occupancy of the crystal orientation <001>, respectively. On the other hand, in the oxide semiconductor film of the comparative example, the occupancy of the crystal orientation <101> and the occupancy of the crystal orientation <111> are 4.2 times and 3.5 times the occupancy of the crystal orientation <001>, respectively.

[0118] The distribution map of GOS obtained by color-coding a plurality of crystal grains included in the oxide semiconductor film of the embodiment is shown in FIG. Figure 3 In addition, the distribution map of GOS obtained by color-differentiating the plurality of crystal grains based on the GOS of each of the plurality of crystal grains included in the oxide semiconductor film of the comparative example is shown in FIG. Fig.19 In other words, Figure 3 and Fig.19 is a distribution map showing the size of the crystal orientation difference within the grain. Figure 3 and Fig.19 In the figure, the GOS of each of the plurality of crystal grains are distinguished by color based on the color bar shown in the figure. As the color of the crystal grain changes from blue to red, that is, as the wavelength of visible light increases, the crystal orientation difference within the crystal grain increases.

[0119] If Figure 3 The GOS distribution map shown is similar to Fig.19 Compared with the GOS distribution map shown in Fig.19 In the GOS distribution map shown in the figure, multiple grains are distinguished by blue color. Figure 3 In the GOS distribution map shown, there are a mixture of grains differentiated by blue color and grains differentiated by green color. Therefore, it can be seen that the oxide semiconductor film of the embodiment contains a large number of grains with large changes in crystal orientation compared to the oxide semiconductor film of the comparative example. Figure 2 In the IPF map shown, gradation of color within the crystal grains can also be confirmed, and it can be seen that a large number of crystal grains with large changes in crystal orientation are included.

[0120] The average GOS values ​​in the measurement region were calculated. As a result, the average GOS values ​​of the oxide semiconductor film of the example and the oxide semiconductor film of the comparative example were 3.89° and 0.71°, respectively.

[0121] Information related to the crystal structures of the oxide semiconductor films of the embodiment and the oxide semiconductor films of the comparative example is shown in Table 3. As shown in Table 3, the oxide semiconductor films of the embodiment and the oxide semiconductor films of the comparative example have the same crystal structure of the bixbyite structure, but the characteristics of the crystal orientation of the crystal grains contained in each are greatly different.

[0122] [Table 3]

[0123] Example Comparative Example Crystal structure Bixbyite-type structure Bixbyite-type structure Average crystal particle size (μm) 0.61 0.65 Maximum crystal size (μm) 1.1 1.1 Crystal orientation <001> Share of (%) 1.8 5.6 Crystal orientation <101> Share of (%) 14.7 23.3 Crystal orientation <111> Share of (%) 39.2 19.8 GOS mean value (°) 3.89 0.71

[0124] As described above, the oxide semiconductor film involved in this embodiment has significant characteristics in the crystal orientation of the grains and has a new crystal structure different from the existing oxide semiconductor. The thin film transistor using the oxide semiconductor film involved in this embodiment has a high field effect mobility compared to the thin film transistor using the existing oxide semiconductor film, and the details will be described later. Therefore, it is speculated that the oxide semiconductor film involved in this embodiment itself also has a high mobility.

[0125] <Second embodiment>

[0126] Reference Figures 4 to 13 A thin film transistor according to one embodiment of the present invention will be described. The thin film transistor according to this embodiment can be used in, for example, a display device, an integrated circuit (IC) such as a microprocessor (Micro-Processing Unit: MPU), or a memory circuit.

[0127] [1. Configuration of Thin Film Transistor 10]

[0128] Figure 4 1 is a cross-sectional view schematically showing a thin film transistor 10 according to an embodiment of the present invention. Figure 5 It is a plan view schematically showing a thin film transistor 10 according to an embodiment of the present invention.

[0129] like Figure 4 As shown, the thin film transistor 10 is provided on a substrate 100. The thin film transistor 10 includes a gate electrode 105, gate insulating layers 110 and 120, an oxide semiconductor layer 140, a gate insulating layer 150, a gate electrode 160, insulating layers 170 and 180, a source electrode 201, and a drain electrode 203. When the source electrode 201 and the drain electrode 203 are not particularly distinguished, they are sometimes collectively referred to as source / drain electrodes 200.

[0130] The gate electrode 105 is provided on the substrate 100. The gate insulating layers 110 and 120 are provided on the substrate 100 and the gate electrode 105. The oxide semiconductor layer 140 is provided on the gate insulating layer 120. The oxide semiconductor layer 140 is in contact with the gate insulating layer 120. The surface of the main surface of the oxide semiconductor layer 140 that is in contact with the gate insulating layer 120 is referred to as a lower surface 142.

[0131] The gate electrode 160 is opposite to the oxide semiconductor layer 140. The gate insulating layer 150 is provided between the oxide semiconductor layer 140 and the gate electrode 160. The gate insulating layer 150 is in contact with the oxide semiconductor layer 140. The surface in contact with the gate insulating layer 150 among the main surfaces of the oxide semiconductor layer 140 is referred to as an upper surface 141. The surface between the upper surface 141 and the lower surface 142 is referred to as a side surface 143. The insulating layers 170 and 180 are provided on the gate insulating layer 150 and the gate electrode 160. The insulating layers 170 and 180 are provided with openings 171 and 173 for exposing the oxide semiconductor layer 140. The source electrode 201 is provided in a manner filling the inside of the opening 171. The source electrode 201 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 171. The drain electrode 203 is provided in a manner filling the inside of the opening 173. The drain electrode 203 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 173.

[0132] The gate electrode 105 has a function as a bottom gate of the thin film transistor 10 and a function as a light shielding film for the oxide semiconductor layer 140. The gate insulating layer 110 has a function as a blocking film for shielding impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140. The gate insulating layers 110 and 120 have a function as gate insulating layers for the bottom gate.

[0133] The oxide semiconductor layer 140 is divided into a source region S, a drain region D, and a channel region CH. The channel region CH is a region vertically below the gate electrode 160 in the oxide semiconductor layer 140. The source region S is a region of the oxide semiconductor layer 140 that does not overlap with the gate electrode 160, and is a region closer to the source electrode 201 than the channel region CH. The drain region D is a region of the oxide semiconductor layer 140 that does not overlap with the gate electrode 160, and is a region closer to the drain electrode 203 than the channel region CH. The oxide semiconductor layer 140 in the channel region CH has physical properties as a semiconductor. The oxide semiconductor layer 140 in the source region S and the drain region D has physical properties as a conductor.

[0134] The gate electrode 160 has the function of serving as the top gate of the thin film transistor 10 and a light shielding film for the oxide semiconductor layer 140. The gate insulating layer 150 has the function of serving as a gate insulating layer for the top gate and has the function of releasing oxygen through heat treatment in the manufacturing process. The insulating layers 170 and 180 have the function of insulating the gate electrode 160 from the source / drain electrode 200 to reduce the parasitic capacitance therebetween. The operation of the thin film transistor 10 is mainly controlled by the voltage supplied to the gate electrode 160. An auxiliary voltage is supplied to the gate electrode 105. However, in the case where the gate electrode 105 is used only as a light shielding film, it is also possible to float the gate electrode 105 instead of supplying a specific voltage. That is, the gate electrode 105 may also be simply referred to as a "light shielding film".

[0135] In this embodiment, a dual-gate transistor in which gate electrodes are provided both above and below the oxide semiconductor layer is used as the thin film transistor 10, but the present invention is not limited to this configuration. For example, a bottom-gate transistor in which a gate electrode is provided only below the oxide semiconductor layer 140 or a top-gate transistor in which a gate electrode is provided only above the oxide semiconductor layer 140 may be used as the thin film transistor 10. The above configuration is only one embodiment, and the present invention is not limited to the above configuration.

[0136] like Figure 5 As shown, in the D1 direction, the width of the gate electrode 105 is greater than the width of the gate electrode 160. The D1 direction is a direction connecting the source electrode 201 and the drain electrode 203, and is a direction indicating the channel length L of the thin film transistor 10. Specifically, the length in the D1 direction of the region (channel region CH) where the oxide semiconductor layer 140 and the gate electrode 160 overlap is the channel length L, and the width in the D2 direction of the channel region CH is the channel width W.

[0137] In this embodiment, the gate insulating layer 150 is formed on the entire surface and the openings 171 and 173 are provided in the gate insulating layer 150, but the present invention is not limited to this configuration. The gate insulating layer 150 may also be patterned. For example, the gate insulating layer 150 may be patterned so that not only the upper surface of the oxide semiconductor layer 140 but also the side surface of the oxide semiconductor layer 140 is exposed.

[0138] exist Figure 5 , the structure in which the source / drain electrode 200 does not overlap with the gate electrodes 105 and 160 in a plan view is illustrated, but the present invention is not limited to this structure. For example, the source / drain electrode 200 may overlap with at least one of the gate electrodes 105 and 160 in a plan view. The above structure is only one embodiment, and the present invention is not limited to the above structure.

[0139] [2. Materials of Components of the Thin Film Transistor 10]

[0140] As the substrate 100, a glass substrate, a quartz substrate, a sapphire substrate, or other light-transmitting rigid substrate is used. When the substrate 100 needs to be flexible, a substrate containing resin such as a polyimide substrate, an acrylic substrate, a siloxane-based substrate, or a fluororesin substrate can be used as the substrate 100. When a substrate containing resin is used as the substrate 100, impurities may be introduced into the above-mentioned resin in order to improve the heat resistance of the substrate 100. In the case where the thin film transistor 10 is a pixel transistor included in a display device such as a top emission type OLED, the substrate 100 does not need to be transparent, so impurities that reduce the transparency of the substrate 100 may also be used. In the case where the thin film transistor 10 is used in an integrated circuit that is not a display device, as the substrate 100, a semiconductor substrate such as a silicon substrate, a silicon carbide substrate, a compound semiconductor substrate, or a conductive substrate such as a stainless steel substrate that is not light-transmitting is used.

[0141] A common metal material is used as the gate electrode 105, the gate electrode 160, and the source / drain electrode 200. For example, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys or compounds thereof are used as these members. The gate electrode 105, the gate electrode 160, and the source / drain electrode 200 may be used in a single layer or in a stacked layer.

[0142] As the gate insulating layers 110 and 120 and the insulating layers 170 and 180, a general insulating layer material is used. For example, silicon oxide (SiO x ), silicon oxynitride (SiO x Ny ), silicon nitride (SiN x ), silicon oxynitride (SiN x O y ), aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ), aluminum oxynitride (AlN x O y ), aluminum nitride (AlN x ) and other inorganic insulating layers.

[0143] As the gate insulating layer 150, an insulating layer containing oxygen among the above insulating layers is used. For example, as the gate insulating layer 150, silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ) and other inorganic insulating layers.

[0144] An insulating layer having a function of releasing oxygen by heat treatment is used as the gate insulating layer 120. The temperature of the heat treatment for releasing oxygen from the gate insulating layer 120 is, for example, 600° C. or less, 500° C. or less, 450° C. or less, or 400° C. or less. That is, the gate insulating layer 120 releases oxygen at a heat treatment temperature performed in a manufacturing process of the thin film transistor 10 when a glass substrate is used as the substrate 100, for example.

[0145] As the gate insulating layer 150, an insulating layer with few defects is used. For example, when the composition ratio of oxygen in the gate insulating layer 150 is compared with the composition ratio of oxygen in an insulating layer having the same composition as the gate insulating layer 150 (hereinafter referred to as "another insulating layer"), the composition ratio of oxygen in the gate insulating layer 150 is closer to the stoichiometric ratio of the insulating layer than the composition ratio of oxygen in the other insulating layer. Specifically, silicon oxide (SiO x ), the oxygen composition ratio of silicon oxide used as the gate insulating layer 150 is closer to the stoichiometric ratio of silicon oxide than the oxygen composition ratio of silicon oxide used as the insulating layer 180. For example, as the gate insulating layer 150, a layer in which no defects are observed when evaluated by an electron spin resonance method (ESR) may be used.

[0146] The above SiO x N y and AlO x N yIt is a silicon compound or aluminum compound containing nitrogen (N) at a ratio (x>y) less than oxygen (O). x O y and AlN x O y These are silicon compounds and aluminum compounds containing oxygen at a ratio smaller than that of nitrogen (x>y).

[0147] The oxide semiconductor film according to the first embodiment can be used as the oxide semiconductor layer 140. The oxide semiconductor layer 140 has crystallinity. Crystalline oxide semiconductors are less likely to form oxygen vacancies than amorphous oxide semiconductors. However, the oxide semiconductor layer 140 may include an amorphous region at a grain boundary.

[0148] [3. Method for Manufacturing Thin Film Transistor 10]

[0149] Figure 6 1 is a flowchart showing a method for manufacturing the thin film transistor 10 according to one embodiment of the present invention. Figure 7 to Figure 13 It is a cross-sectional view showing a method for manufacturing the thin film transistor 10 according to one embodiment of the present invention.

[0150] like Figure 6 and Figure 7 As shown, a gate electrode 105 serving as a bottom gate is formed on a substrate 100, and gate insulating layers 110 and 120 are formed on the gate electrode 105 ( Figure 6 The gate insulating layer 110 may be formed of silicon nitride, for example. The gate insulating layer 120 may be formed of silicon oxide, for example. The gate insulating layers 110 and 120 are formed by CVD (Chemical Vapor Deposition).

[0151] By using silicon nitride as the gate insulating layer 110, the gate insulating layer 110 can block, for example, impurities diffusing from the substrate 100 side toward the oxide semiconductor layer 140. Silicon oxide used as the gate insulating layer 120 has a property of releasing oxygen by heat treatment.

[0152] like Figure 6 and Figure 8 As shown, an oxide semiconductor layer 140 ( Figure 6 In this process, an oxide semiconductor layer 140 may be formed on the substrate 100. The oxide semiconductor layer 140 is formed by a sputtering method.

[0153] The thickness of the oxide semiconductor layer 140 is, for example, not less than 10 nm and not more than 100 nm, not less than 15 nm and not more than 70 nm, or not less than 20 nm and not more than 40 nm. The oxide semiconductor layer 140 before heat treatment (OS annealing) described later is amorphous.

[0154] When the oxide semiconductor layer 140 is crystallized by OS annealing described later, the oxide semiconductor layer 140 after film formation and before OS annealing is preferably amorphous (a state in which the crystalline component of the oxide semiconductor is small). That is, the film formation conditions of the oxide semiconductor layer 140 are preferably conditions in which the oxide semiconductor layer 140 is not crystallized as much as possible immediately after film formation. For example, when the oxide semiconductor layer 140 is formed by sputtering, the oxide semiconductor layer 140 is formed while the temperature of the object to be film-formed (the substrate 100 and the structure formed thereon) is controlled to be 100° C. or less.

[0155] like Figure 6 and Fig. 9 As shown, the pattern of the oxide semiconductor layer 140 is formed ( Figure 6 Although not shown in the figure, a reagent-resistant mask is formed on the oxide semiconductor layer 140, and the oxide semiconductor layer 140 is etched using the reagent-resistant mask. The oxide semiconductor layer 140 can be etched by wet etching or dry etching. As wet etching, an acidic etchant can be used for etching. As an etchant, oxalic acid or hydrofluoric acid can be used, for example.

[0156] After the patterning of the oxide semiconductor layer 140, the oxide semiconductor layer 140 is subjected to a heat treatment (OS annealing) ( Figure 6 In this embodiment, the oxide semiconductor layer 140 is crystallized by the OS annealing.

[0157] like Figure 6 and Fig.10 As shown, a gate insulating layer 150 is formed on the oxide semiconductor layer 140 ( Figure 6 ("GI formation" in step S3005). As the gate insulating layer 150, for example, silicon oxide is formed. The gate insulating layer 150 is formed by a CVD method. For example, in order to form an insulating layer with few defects as described above as the gate insulating layer 150, the gate insulating layer 150 may be formed at a film forming temperature of 350°C or higher. The thickness of the gate insulating layer 150 is, for example, not less than 50nm and not more than 300nm, not less than 60nm and not more than 200nm, or not less than 70nm and not more than 150nm. After the gate insulating layer 150 is formed, a process of injecting oxygen into a portion of the gate insulating layer 150 may be performed.

[0158] In a state where the gate insulating layer 150 is formed on the oxide semiconductor layer 140, heat treatment (oxidation annealing) for supplying oxygen to the oxide semiconductor layer 140 is performed ( Figure 6 In the process from forming the oxide semiconductor layer 140 to forming the gate insulating layer 150 on the oxide semiconductor layer 140, a large number of oxygen vacancies are generated on the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. Through the above-mentioned oxidation annealing, oxygen released from the gate insulating layers 120 and 150 is supplied to the oxide semiconductor layer 140 to repair the oxygen vacancies.

[0159] like Figure 6 and Fig.11 As shown, a gate electrode 160 is formed on the gate insulating layer 150 ( Figure 6 The gate electrode 160 is formed by sputtering or atomic layer deposition and patterned by photolithography. The gate electrode 160 is formed in contact with the gate insulating layer 150 .

[0160] In a state where the gate electrode 160 is patterned, the resistance of the source region S and the drain region D of the oxide semiconductor layer 140 is reduced ( Figure 6 Specifically, impurities are injected into the oxide semiconductor layer 140 from the gate electrode 160 side through the gate insulating layer 150 by ion implantation. By ion implantation, for example, argon (Ar), phosphorus (P), and boron (B) are injected into the oxide semiconductor layer 140. Oxygen vacancies are formed in the oxide semiconductor layer 140 by ion implantation, thereby reducing the resistance of the oxide semiconductor layer 140. Since the gate electrode 160 is provided above the oxide semiconductor layer 140 that functions as the channel region CH of the thin film transistor 10, impurities are not injected into the oxide semiconductor layer 140 in the channel region CH.

[0161] like Figure 6 and Fig.12 As shown, insulating layers 170 and 180 are formed on the gate insulating layer 150 and the gate electrode 160 as interlayer films ( Figure 6 The insulating layers 170 and 180 are formed by CVD. For example, silicon nitride is formed as the insulating layer 170, and silicon oxide is formed as the insulating layer 180. The materials used for the insulating layers 170 and 180 are not limited to the above. The thickness of the insulating layer 170 is not less than 50 nm and not more than 500 nm. The thickness of the insulating layer 180 is not less than 50 nm and not more than 500 nm.

[0162] like Figure 6 and Fig.13As shown, openings 171 and 173 are formed in the gate insulating layer 150 and the insulating layers 170 and 180 ( Figure 6 The oxide semiconductor layer 140 in the source region S is exposed through the opening 171. The oxide semiconductor layer 140 in the drain region D is exposed through the opening 173. The source / drain electrode 200 ( Figure 6 Step S3011 of "SD formation"), thereby completing Figure 4 The thin film transistor 10 is shown.

[0163] In the thin film transistor 10 manufactured by the above manufacturing method, a mobility of 30 [cm 2 / Vs] or more, 35[cm 2 / Vs] or more or 40[cm 2 / Vs] or above. It should be noted that the mobility in this embodiment is the field effect mobility in the saturation region of the thin film transistor 10, which refers to the maximum value of the field effect mobility in the region where the potential difference (Vd) between the source electrode and the drain electrode is greater than the value (Vg-Vth) obtained by subtracting the threshold voltage (Vth) of the thin film transistor 10 from the voltage (Vg) supplied to the gate electrode.

[0164] Furthermore, cross-sectional STEM (Scanning Transmission Electron Microscopy) observation of the thin film transistor 10 manufactured by the above-mentioned manufacturing method was performed. Fig.14 and Fig.15 It is a cross-sectional STEM image of the thin film transistor 10 according to one embodiment of the present invention. Fig.14 The regions (a) to (c) surrounded by rectangles in FIG. 1 are regions including the oxide semiconductor layer OS. Fig.15 These are cross-sectional STEM images of the enlarged regions (a) to (c).

[0165] like Fig.15 As shown, in any region of regions (a) to (c), no grain boundary in the oxide semiconductor layer OS can be confirmed in the film thickness direction. That is, in at least a portion of the region of the oxide semiconductor layer OS, a portion of the upper surface and a portion of the lower surface of the oxide semiconductor layer OS are formed by one crystal grain. In other words, the oxide semiconductor layer OS has a continuous crystal structure in the film thickness direction.

[0166] <Third embodiment>

[0167] Reference Fig.16 An electronic device according to an embodiment of the present invention will be described.

[0168] Fig.16 1 is a schematic diagram showing an electronic device 1000 according to an embodiment of the present invention. Fig.16 , a smartphone is shown as an example of the electronic device 1000. The electronic device 1000 includes a display device 1100 with a curved side. The display device 1100 includes a plurality of pixels for displaying an image, and the plurality of pixels are controlled by a pixel circuit and a driving circuit. The pixel circuit and the driving circuit include the thin film transistor 10 described in the second embodiment. Since the thin film transistor 10 has a high field effect mobility, the responsiveness of the pixel circuit and the driving circuit can be improved, and as a result, the performance of the electronic device 1000 can be improved.

[0169] It should be noted that the electronic device 1000 involved in this embodiment is not limited to a smartphone. The electronic device 1000 also includes, for example, an electronic device having a display device such as a watch, a tablet computer, a laptop computer, a car navigation system, or a television. In addition, the oxide semiconductor film described in the first embodiment or the thin film transistor 10 described in the second embodiment can be applied to all electronic devices regardless of whether there is a display device or not.

[0170] The various embodiments described above as embodiments of the present invention can be appropriately combined and implemented as long as they do not contradict each other. In addition, solutions obtained by adding, deleting or designing components or adding, omitting or changing conditions of processes based on the various embodiments by those skilled in the art are also included in the scope of the present invention as long as they have the gist of the present invention.

[0171] Even if there are other effects different from the effects brought about by the schemes of the above-mentioned embodiments, if they are clearly known from the description of this specification or can be easily predicted by those skilled in the art, they are of course understood to be the effects brought about by the present invention.

[0172] Description of Reference Numerals

[0173] 10: thin film transistor, 100: substrate, 105, 160: gate electrode, 110, 120, 150: gate insulating layer, 140: oxide semiconductor layer, 141: upper surface, 142: lower surface, 143: side surface, 170, 180: insulating layer, 171, 173: opening, 200: source / drain electrode, 201: source electrode, 203: drain electrode, 1000: electronic device, 1100: display device

Claims

1. An oxide semiconductor film, which is a crystalline oxide semiconductor film provided on a substrate, wherein: The oxide semiconductor film includes: Indium (In) element; and a first metal (M1) element selected from the group consisting of aluminum (Al), gallium (Ga), yttrium (Y), scandium (Sc) and lanthanide elements, The oxide semiconductor film includes a plurality of crystal grains, each of the plurality of crystal grains including at least one of a crystal orientation of <001>, a crystal orientation of <101>, and a crystal orientation of <111> obtained by an EBSD (electron backscatter diffraction) method, Among the occupancy rates of the crystal orientation calculated based on the measurement points of the crystal orientation having a crystal orientation difference of 0° to 15° relative to the normal direction of the surface of the substrate, the occupancy rate of the crystal orientation <111> is greater than the occupancy rate of the crystal orientation <001> and the occupancy rate of the crystal orientation <101>.

2. The oxide semiconductor film according to claim 1, wherein The occupancy rate of the crystal orientation <101> is greater than the occupancy rate of the crystal orientation <001>.

3. The oxide semiconductor film according to claim 1, wherein The occupancy rate of the crystal orientation <101> is 4.5 times or more the occupancy rate of the crystal orientation <001>.

4. The oxide semiconductor film according to claim 1, wherein The occupancy rate of the crystal orientation <111> is 4 times or more the occupancy rate of the crystal orientation <001>.

5. The oxide semiconductor film according to claim 1, wherein The average GOS value of the plurality of crystal grains is greater than or equal to 2°.

6. The oxide semiconductor film according to claim 1, wherein One of the crystal grains forms a portion of the lower surface and a portion of the upper surface of the oxide semiconductor film.

7. The oxide semiconductor film according to any one of claims 1 to 6, wherein The atomic ratio of the indium element and the metal element (M) other than the indium element satisfies the formula (1): [Mathematical formula 1] 8. The oxide semiconductor film according to any one of claims 1 to 6, wherein The first metal element is the gallium element, The oxide semiconductor film further includes a second metal (M2) element selected from the group consisting of the aluminum element, the yttrium element, the scandium element, and the lanthanide element, The atomic ratio of the indium element, the gallium element and the second metal element satisfies formula (2), formula (3) and formula (4): [Mathematical formula 2] [Mathematical formula 3] [Formula 4] 9 . A thin film transistor comprising the oxide semiconductor film according to claim 1 as a channel.

10. An electronic device comprising the thin film transistor according to claim 9.