3D printing integrated bionic stent as well as preparation method and application thereof

By using 3D printed integrated bionic scaffolds prepared with polyterephthalate-butylene adipate and other materials, the problems of low compressive strength in early bone formation and slow degradation in late stages were solved, and rapid within three months was achieved Degradation and new bone growth promote bone repair and reduce inflammatory response.

CN118873753APending Publication Date: 2024-11-01NORTHEAST NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410961222.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing 3D printed bone stents have low compressive strength in the early stage of bone formation and slow degradation in the later stage, which hinders the generation of new bone.

Method used

Using a combination of polyterephthalate-butylene adipate, calcium chloride, strontium chloride, sodium alginate and sodium percarbonate, 3D printed integrated bionic scaffolds are prepared by mixing and drying to provide early mechanical support. And it degrades rapidly within two months to promote the growth of new bone.

Benefits of technology

Provide appropriate compressive strength in the early stage of bone formation and significantly degrade within three months, without hindering new bone formation, while promoting new bone growth and reducing inflammatory response, significantly improving the bone repair effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118873753A_ABST
    Figure CN118873753A_ABST
Patent Text Reader

Abstract

The invention provides a 3D printing integrated bionic stent and a preparation method and application thereof, and belongs to the technical field of medical materials. The invention provides a 3D printing integrated bionic scaffold. The 3D printing integrated bionic scaffold comprises the following components in parts by mass: 80 parts of poly (butylene terephthalate)-adipate, 1-4 parts of calcium chloride, 1-4 parts of strontium chloride, 2-10 parts of sodium alginate and 1-10 parts of sodium percarbonate. The 3D printing integrated bionic scaffold provided by the invention can provide proper compressive strength in the early stage of bone formation, can be obviously degraded within three months, and cannot hinder the formation of new bones; meanwhile, the growth of new bones can be effectively promoted, and inflammatory response is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical materials, and in particular to a 3D printed integrated bionic scaffold and a preparation method and application thereof. Background Art

[0002] Bone defects are a major challenge in clinical orthopedics. When the size of a bone defect exceeds a critical value, the body loses its ability to heal itself. Today, research on artificial scaffolds to treat bone defects has evolved from developing filling materials to inducing in situ bone reconstruction. Implants should resemble the natural mineral phase of bone and be bioactive. As new bone grows, the scaffold should further gradually degrade. Metal implants are the most commonly used in clinical practice, but they are affected by osteogenic activity, tissue compatibility, and degradation. These devices usually require a second operation to remove, which is inefficient and inconvenient for doctors and patients. Autologous transplantation is considered a good method, but it is also associated with disease and poor availability at the harvesting site. Allografts (tissues obtained from human cadavers or living donors) and xenografts (tissues derived from a species different from the specimen recipient) have the risk of excessive immune response, leading to transplant rejection. As a surgical procedure, reconstruction of bone tissue defects is a time-consuming and technically difficult process that does not always achieve the desired results, exposing patients to residual pain, nonunion, or refractory infection.

[0003] 3D printed bone scaffolds have the potential to replace autologous grafts and allografts because of their advantages such as unlimited supply and customized scaffold biochemical, biological and biophysical properties. Currently available synthetic bone substitutes in the clinic generally perform well in some characteristics but poorly in others. For example, synthetic grafts made of calcium phosphate and bioactive glass can provide good bone tissue integration but lack mechanical strength, especially toughness, while metal scaffolds are mechanically stable but often have poor integration with in vivo tissues. Polybutylene terephthalate-adipate (PBAT) is a relatively new polymer with low crystallinity, attractive biodegradability and mechanical properties, suitable for orthopedic applications. However, its in vivo degradation time is too slow, which can easily hinder new bone formation; alginate hydrogels have the advantages of good biocompatibility, excellent plasticity and wide sources. They can be used as excellent carriers of cells and growth factors and are widely used in bone tissue engineering research. Alginate hydrogels generally have problems such as poor mechanical strength, fast degradation time or insufficient osteoinduction ability. That is, the 3D printed bone scaffolds in the prior art have the problems of low compressive strength in the early stage of bone formation and slow degradation in the later stage, which hinders the formation of new bone. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a 3D printed integrated bionic scaffold and its preparation method and application. The 3D printed integrated bionic scaffold of the present invention provides appropriate compressive strength in the early stage of bone formation, and can be significantly degraded within two months without hindering the formation of new bone.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a 3D printed integrated bionic scaffold, comprising the following components in parts by mass:

[0007] 80 parts of polybutylene terephthalate-adipate, 1-4 parts of calcium chloride, 1-4 parts of strontium chloride, 2-10 parts of sodium alginate and 1-10 parts of sodium percarbonate.

[0008] Preferably, the 3D printed integrated bionic scaffold comprises the following components in parts by weight:

[0009] 80 parts of polybutylene terephthalate-adipate, 3 parts of calcium chloride, 3 parts of strontium chloride, 10 parts of sodium alginate and 2 parts of sodium percarbonate.

[0010] Preferably, the 3D printed integrated bionic scaffold comprises the following components in parts by weight:

[0011] 80 parts of polybutylene terephthalate-adipate, 1 part of calcium chloride, 1 part of strontium chloride, 10 parts of sodium alginate and 2 parts of sodium percarbonate.

[0012] Preferably, the 3D printed integrated bionic scaffold comprises the following components in parts by weight:

[0013] 80 parts of polybutylene terephthalate-adipate, 3 parts of calcium chloride, 3 parts of strontium chloride, 10 parts of sodium alginate and 1 part of sodium percarbonate.

[0014] The present invention also provides a method for preparing the 3D printed integrated bionic scaffold described in the above technical solution, comprising the following steps:

[0015] Polybutylene terephthalate-adipate, calcium chloride, strontium chloride, sodium alginate, sodium percarbonate and an organic solvent are mixed and dried to obtain the 3D printed integrated bionic scaffold.

[0016] Preferably, the organic solvent is chloroform.

[0017] Preferably, the mass of the chloroform is 10% of the mass of the polybutylene terephthalate-adipate.

[0018] The present invention also provides the use of the 3D printed integrated bionic scaffold described in the above technical solution in the preparation of 3D printed integrated materials for bone regeneration.

[0019] Preferably, the application comprises the following steps: 3D printing the 3D printed integrated bionic scaffold, the 3D printing speed is 5 mm / s, the extrusion pressure is 240 MPa, and the printing temperature is 180-210°C.

[0020] The present invention provides a 3D printed integrated bionic scaffold, comprising the following components in parts by mass:

[0021] 80 parts of polybutylene terephthalate-adipate, 1-4 parts of calcium chloride, 1-4 parts of strontium chloride, 2-10 parts of sodium alginate and 1-10 parts of sodium percarbonate.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] In-situ self-fixation and accelerated degradation performance

[0024] PBAT is a completely biocompatible and biodegradable aromatic copolyester. The present invention combines PBAT with a hydrogel material. The PBAT main material provides a porous printing structure to play a mechanical support role. The sodium alginate, calcium chloride and strontium chloride mixed therein and co-printed form a hydrogel that swells after absorbing tissue exudate to achieve in situ fixation. At the same time, this process gradually loosens and degrades the polymer itself, so that it meets the mechanical properties in the early stage after implantation in the body, has a porous structure, slowly releases active factors, and rapidly degrades in the later stage, becoming a high-performance composite material; based on the advantages of good biocompatibility, excellent plasticity, and a wide range of sources, alginate hydrogel can provide an excellent carrier for cells and growth factors, and is widely used in the study of bone tissue engineering. At the same time, the strontium chloride, calcium chloride and sodium percarbonate incorporated therein are inorganic salt ions, which can be well integrated into the human body, which is conducive to early bone repair and regulation of the inflammatory microenvironment.

[0025] Oxygen release function

[0026] The release of oxygen through the peroxide salt sodium percarbonate can alleviate the hypoxic microenvironment and stimulate macrophage polarization to M2. Since M2 macrophages have the function of inhibiting inflammatory response, promoting tissue remodeling and wound healing, they can promote bone repair. In addition, long-term hypoxia in chronic wounds can negatively affect the formation of vascular endothelial growth factor (VEGF), thereby interfering with angiogenesis and wound closure. The oxygen released by adding sodium percarbonate can effectively eliminate this negative impact.

[0027] Bone repair, promote blood vessel growth

[0028] Sodium alginate contains a large number of carboxyl groups and can exhibit polycationic behavior in aqueous solution. It can quickly form hydrogels with multivalent cations under relatively mild conditions. When divalent cations such as calcium ions and strontium ions are present, the sodium ions on α-L-guluronic acid undergo ion exchange reactions with divalent cations to quickly form a cross-linked network structure, thereby forming a hydrogel. Strontium ions have the function of promoting osteogenesis and angiogenesis. Strontium has the function of promoting osteogenesis and inhibiting osteoclasts, and can promote angiogenesis, etc.

[0029] In summary, the 3D printed integrated bionic scaffold provided by the present invention can provide appropriate compressive strength in the early stage of bone formation, and can be significantly degraded within three months without hindering the formation of new bone; at the same time, it can effectively promote new bone growth and reduce inflammatory response. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 are the XRD patterns of different groups;

[0031] Figure 2 This is a diagram showing the oxygen release effect of the 3D printed integrated bionic scaffold prepared in Example 1;

[0032] Figure 3 This is the oxygen release curve of the 3D printed integrated bionic scaffold prepared in Example 1;

[0033] Figure 4 This is the test curve of compression strength changing with degradation time;

[0034] Figure 5 It is a bar graph of the healing area of ​​rat skull defects;

[0035] Figure 6 HE and Masson images of skull sections of rats in different groups at 12 weeks;

[0036] Figure 7 Staining for alkaline phosphatase ALP;

[0037] Figure 8 This is the immunohistochemical staining of CD31 in endothelial cells;

[0038] Fig. 9 Live / dead staining of mouse osteoblast MC3T3 cells. DETAILED DESCRIPTION

[0039] The present invention provides a 3D printed integrated bionic scaffold, comprising the following components in parts by mass:

[0040] 80 parts of polybutylene terephthalate-adipate, 1-4 parts of calcium chloride, 1-4 parts of strontium chloride, 2-10 parts of sodium alginate and 1-10 parts of sodium percarbonate.

[0041] In the present invention, unless otherwise specified, the raw materials used are all commercially available products in the art.

[0042] In the present invention, the 3D printed integrated bionic scaffold preferably includes the following components in parts by mass:

[0043] 80 parts of polybutylene terephthalate-adipate, 3 parts of calcium chloride, 3 parts of strontium chloride, 10 parts of sodium alginate and 2 parts of sodium percarbonate;

[0044] Or preferably include the following components in parts by weight:

[0045] 80 parts of polybutylene terephthalate-adipate, 1 part of calcium chloride, 1 part of strontium chloride, 10 parts of sodium alginate and 2 parts of sodium percarbonate;

[0046] Or preferably include the following components in parts by weight:

[0047] 80 parts of polybutylene terephthalate-adipate, 3 parts of calcium chloride, 3 parts of strontium chloride, 10 parts of sodium alginate and 1 part of sodium percarbonate.

[0048] The present invention also provides a method for preparing the 3D printed integrated bionic scaffold described in the above technical solution, comprising the following steps:

[0049] Polybutylene terephthalate-adipate, calcium chloride, strontium chloride, sodium alginate, sodium percarbonate and an organic solvent are mixed and dried to obtain the 3D printed integrated bionic scaffold.

[0050] In the present invention, the organic solvent is preferably chloroform.

[0051] In the present invention, the mass of the chloroform is preferably 10% of the mass of the polybutylene terephthalate-adipate.

[0052] The present invention adds the PBAT and the organic solvent into a round-bottom flask, and heats and refluxes for 6 hours at 45° C. to fully dissolve, then sequentially adds the sodium alginate, calcium chloride and strontium chloride into the solution, stirs for 2 hours at 350 r / min with a magnetic stirrer, ultrasonicates for 30 minutes, mixes evenly, and finally adds the sodium percarbonate. After stirring evenly, the solution is concentrated by rotary evaporation at 30° C., and the obtained mixed solution is precipitated in cold anhydrous ethanol, and then the solvent is drained in a vacuum oven at 60-65° C. to obtain the 3D printed integrated bionic scaffold.

[0053] The present invention also provides the use of the 3D printed integrated bionic scaffold described in the above technical solution in the preparation of 3D printed integrated materials for bone regeneration.

[0054] In the present invention, the application preferably includes the following steps: 3D printing the 3D printed integrated bionic scaffold, the 3D printing speed is preferably 5 mm / s, the extrusion pressure is preferably 240 MPa, and the printing temperature is preferably 180-210°C.

[0055] The present invention preferably cuts the 3D printing integrated bionic bracket into pieces and adds the pieces into the barrel of a 3D printer, sets printing parameters, and performs the 3D printing.

[0056] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0057] Polybutylene terephthalate-adipate (PBAT), sodium alginate, strontium chloride (SrCl2), calcium chloride (CaCl2), sodium percarbonate, chloroform, anhydrous ethanol, etc. are all from Aladdin Reagent Company.

[0058] Comparative Example 1

[0059] PBAT was dissolved in chloroform (10% wt), heated under reflux for 6 h, and the solution was concentrated by rotary evaporation, precipitated in cold ether, and the solvent was dried in a vacuum oven at 60° C. The obtained solid was cut into pieces, added to the barrel of a 3D printer, and printed according to the set parameters to obtain a comparative example 1 bracket.

[0060] Comparative Example 2

[0061] 80 parts by weight of PBAT were dissolved in chloroform (10% wt), heated and refluxed for 6 hours, and then 10 parts by weight of sodium alginate were added to the solution, stirred for 2 hours by a magnetic stirrer at 350 r / min and ultrasonically mixed, and the solution was concentrated by rotary evaporation at 30°C. Then, the obtained mixed solution was precipitated in anhydrous ethanol, and the solvent was drained in a vacuum oven at 60°C. The obtained solid was cut into pieces, added to the barrel of a 3D printer, and printed according to the set parameters to obtain a comparative example 2 bracket.

[0062] Comparative Example 3

[0063] 80 parts by weight of PBAT were dissolved in chloroform (10% wt), heated under reflux for 6 hours, and then 10 parts by weight of sodium alginate, 3 parts by weight of calcium chloride, and 3 parts by weight of strontium chloride were added to the solution, stirred for 2 hours by a magnetic stirrer at 350 r / min and ultrasonically mixed, and the solution was concentrated by rotary evaporation at 30°C. Then, the obtained mixed solution was precipitated in anhydrous ethanol, and the solvent was drained in a vacuum oven at 60°C. The obtained solid was cut into pieces, added to the barrel of a 3D printer, and printed according to the set parameters to obtain a comparative example 3 bracket.

[0064] Example 1

[0065] 80 parts by weight of PBAT were dissolved in chloroform (10% wt), heated under reflux for 6 hours, and then 10 parts by weight of sodium alginate, 3 parts by weight of calcium chloride, 3 parts by weight of strontium chloride and 2 parts by weight of sodium percarbonate were added to the solution, stirred for 2 hours by a magnetic stirrer at 350 r / min and ultrasonically mixed, and the solution was concentrated by rotary evaporation at 30°C. Then, the mixed solution was precipitated in anhydrous ethanol, the solvent was drained in a vacuum oven at 60°C, the obtained solid was cut into pieces, added to the barrel of a 3D printer, and printed according to the set parameters to obtain Example 1 (3D printed integrated bionic scaffold).

[0066] Figure 1 Figure 3 is the XRD diagram of different groups. Through XRD, we can see that each component is blended into the system, among which 32.09° is the characteristic peak of sodium alginate, 35.02° is the characteristic peak of sodium percarbonate, 28.04° and 40.92° are the characteristic peaks of calcium chloride and strontium chloride, respectively, which confirms the successful doping of each component.

[0067] Since the scaffold is filled with sodium alginate, calcium chloride and strontium chloride, it can form a hydrogel and swell internally when there is tissue exudate at the wound site. According to tests, the swelling rate of the scaffold of Example 1 was 25.16% after being immersed in PBS for 2 hours, and the compressive strength was reduced by 52.14% after being immersed for 3 months, and the degradation rate was significantly accelerated.

[0068] The 3D printed integrated bionic scaffold prepared in Example 1 has a significant oxygen release effect, such as Figure 2 As shown, when it is immersed in PBS buffer, a large number of oxygen bubbles can be seen releasing between the pores.

[0069] The oxygen release was tracked and tested. Figure 3 As shown, it is confirmed that the 3D printed integrated bionic scaffold prepared in Example 1 can maintain long-term high-concentration oxygen release.

[0070] 1cm after printing 3 The cube is used to measure the compressive strength when the compression deformation is 50%, and the pressing speed is 1mm / min. Figure 4As shown, after three months of immersion, the compressive strength of Comparative Example 1 decreased from 10.7MPa to 7.1MPa, and the scaffold degradation was not obvious. The compressive strength of Comparative Example 2 decreased from 8.8MPa to 4.2MPa, and the degradation rate was relatively fast. The degradation trends of Comparative Example 3 and Example 1 were similar, decreasing from 11.2MPa and 11.6MPa to 6.6MPa and 6.3MPa, respectively, and the degradation rates were all above 50%. The degradation rate could be well matched with the bone growth rate, and the initial strength was significantly higher than that of Comparative Example 2, with better mechanical properties, so Example 1 was selected as the preferred scaffold.

[0071] Rats were divided into a blank group, a comparative example 1 group, a comparative example 2 group, a comparative example 3 group, and an example 1 group. After anesthesia, a full-thickness defect (6 mm in diameter) was made in the cranial region of the rats. The corresponding scaffolds were implanted, and the volume of newly formed bone was measured by Micro-CT at 4 weeks (4W), 8 weeks (8W), and 12 weeks (12W). The results are shown in Figure 2. Figure 5 As shown in the figure, the blank group had a slower bone formation rate. As the active components were added, the bone formation volume of the Example 1 group at three time points was significantly higher than that of the blank group, showing the best bone formation ability. After 12 weeks, the dissected skull was immersed in a light-cured single-component resin to prepare slices for HE and Masson staining. Figure 6 As shown, the amount of new bone formation in the blank group was very small, while the collagen and new bone formation in the Example 1 group were the largest, proving the effective osteogenicity of the scaffold.

[0072] Example 2

[0073] The same as Example 1, the only difference is that the mass parts of the raw materials are: 80 parts of PBAT, 10 parts of sodium alginate, 1 part of calcium chloride, 1 part of strontium chloride and 2 parts of sodium percarbonate, that is, Example 2 is a stent with less calcium chloride and strontium chloride content than Example 1.

[0074] Example 3

[0075] The same as Example 1, the only difference is that the mass parts of the raw materials are: 80 parts of PBAT, 10 parts of sodium alginate, 3 parts of calcium chloride, 3 parts of strontium chloride and 1 part of sodium percarbonate, that is, Example 3 is a scaffold with a lower content of sodium percarbonate component than Example 1.

[0076] The activity of ALP can reflect the ability of osteoblasts to synthesize type I collagen and form bone matrix. ALP expression is a key feature of osteogenic differentiation and an early marker of cell differentiation. Mouse embryonic osteoblast MC3T3 cells were cultured in the extract for 7 days, fixed and stained with BCIP / NBT alkaline phosphatase colorimetric kit for 15 minutes, and the stained cells were photographed with an inverted optical microscope. The results are shown in Figure 2. Figure 7As the inorganic components are gradually added, the purple color gradually deepens. Example 1 shows the darkest color due to the large amount of calcium ions and strontium ions contained in it, while Example 2 shows a lighter purple color than Example 1 due to the reduction of inorganic ion content, which proves that the added calcium and strontium have a good ability to promote osteoblast calcification in vitro.

[0077] CD31 is a cell surface glycoprotein, also known as the endothelial cell attachment molecule, and is one of the important markers of endothelial cells. Immunofluorescence staining is often used to visualize the distribution and location of the target protein. Figure 8 As can be seen from the figure, since Example 3 reduces the sodium percarbonate content, CD31 ( Figure 8 The expression of VEGF and VEGF in the red part (in the middle) was lower than that in Example 1, which proved that oxygen-rich environment is conducive to angiogenesis.

[0078] Live / dead staining was further used to determine the biocompatibility of the scaffold. First, the scaffold was sterilized using ultraviolet light. 1 g of the scaffold was weighed and placed in a 10 mL centrifuge tube, and 10 mL of DMEM culture medium was added thereto. After 24 hours, the culture medium was aspirated and filtered to obtain the extract. MC3T3 was added at 5 × 10 5 The cells / well were seeded at a density of 100 μL on a 6-well culture plate and allowed to attach for 4 h. 100 μL of the extract was added to the wells and placed in the culture plate for co-culture with MC3T3. The staining results are shown in Fig. 9 As shown, MC3T3 cells have good cell compatibility in both the comparative example group and the example group.

[0079] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A 3D printed integrated bionic scaffold, characterized in that: The composition includes the following components in parts by weight: 80 parts of polybutylene terephthalate-adipate, 1-4 parts of calcium chloride, 1-4 parts of strontium chloride, 2-10 parts of sodium alginate and 1-10 parts of sodium percarbonate.

2. The 3D printed integrated bionic scaffold according to claim 1, characterized in that: The composition includes the following components in parts by weight: 80 parts of polybutylene terephthalate-adipate, 3 parts of calcium chloride, 3 parts of strontium chloride, 10 parts of sodium alginate and 2 parts of sodium percarbonate.

3. The 3D printed integrated bionic scaffold according to claim 1, characterized in that: The composition includes the following components in parts by weight: 80 parts of polybutylene terephthalate-adipate, 1 part of calcium chloride, 1 part of strontium chloride, 10 parts of sodium alginate and 2 parts of sodium percarbonate.

4. The 3D printed integrated bionic scaffold according to claim 1, characterized in that: The composition includes the following components in parts by weight: 80 parts of polybutylene terephthalate-adipate, 3 parts of calcium chloride, 3 parts of strontium chloride, 10 parts of sodium alginate and 1 part of sodium percarbonate.

5. The method for preparing the 3D printed integrated bionic scaffold according to any one of claims 1 to 4, characterized in that: The following steps are involved: Polybutylene terephthalate-adipate, calcium chloride, strontium chloride, sodium alginate, sodium percarbonate and an organic solvent are mixed and dried to obtain the 3D printed integrated bionic scaffold.

6. The preparation method according to claim 5, characterized in that: The organic solvent is chloroform.

7. The preparation method according to claim 6, characterized in that: The mass of the chloroform is 10% of the mass of the polybutylene terephthalate-adipate.

8. Use of the 3D printed integrated bionic scaffold according to any one of claims 1 to 4 in the preparation of 3D printed integrated materials for bone regeneration.

9. The use according to claim 8, characterized in that: The method comprises the following steps: 3D printing the 3D printed integrated bionic bracket, wherein the 3D printing speed is 5 mm / s, the extrusion pressure is 240 MPa, and the printing temperature is 180-210°C.