Preparation method of aerogel composite material and aerogel composite material

By performing heated and pressurized solvent replacement and drying in a supercritical high-pressure reactor, the problem of high cost and long time in the prior art is solved, and the efficient preparation of aerogel composite materials is achieved, which is suitable for industrial use. Large-scale production.

CN118874351APending Publication Date: 2024-11-01CHANGSHA RONGLAN MACHINERY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410960701.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-16
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the existing aerogel composite preparation methods, solvent replacement and supercritical drying have high costs and long process time, which seriously restricts production capacity.

Method used

The solvent is replaced and dried by a supercritical high-pressure reactor. The diffusion rate and compatibility of the solvent are significantly improved by heating and pressurization, shortening the replacement time, and directly supercritical drying is carried out to reduce the amount of solvent and process cycle.

Benefits of technology

It greatly shortens the preparation cycle of aerogel and its composite materials, reduces production costs, improves the preparation efficiency, the structural integrity and performance stability of the product, and is suitable for industrial-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004950180450000171
    Figure BDA0004950180450000171
Patent Text Reader

Abstract

The invention relates to the technical field of aerogel composite material preparation, and discloses a preparation method of an aerogel composite material and the aerogel composite material. The preparation method of the aerogel composite material comprises the following steps: S100, putting wet gel into a supercritical high-pressure reactor, carrying out solvent replacement in the supercritical high-pressure reactor, and verifying the air tightness of the supercritical high-pressure reactor by utilizing a solvent replacement process; and S200, directly carrying out supercritical drying in a supercritical high-pressure reactor. The characteristics of a supercritical high-pressure reactor, solvent replacement prepared from an aerogel composite material and a supercritical drying process are fully matched and combined, the supercritical high-pressure reactor is effectively utilized, and the utilization rate of the supercritical high-pressure reactor is increased; therefore, heating and pressurizing for solvent replacement are ensured to improve the safety of solvent replacement, and the air tightness verification process in the supercritical drying process is omitted, so that the preparation time of the whole aerogel composite material is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aerogel composite material preparation, and in particular, to a method for preparing an aerogel composite material. In addition, the present invention also relates to an aerogel composite material prepared by the method for preparing the aerogel composite material. Background Art

[0002] The most commonly used preparation method for preparing aerogel and its composite materials by sol-gel method in the prior art is to go through the processes of aging, solvent replacement and supercritical drying. The purpose of solvent replacement is to replace the water and other reaction impurities in the wet gel to reduce the damage to the aerogel network structure caused by the capillary force in the supercritical drying process.

[0003] The commonly used replacement method currently relies on static replacement of concentration differences, which is mainly achieved by molecular diffusion caused by the concentration gradient between solvents. It requires large amounts of solvents, multiple times, and long replacements to achieve better results. This process consumes a lot of solvents and time, resulting in high process costs and serious restrictions on production capacity.

[0004] Some studies have attempted to increase the replacement speed by raising the temperature and stirring, but the results have been limited. In addition, some studies have used microwave irradiation to perform solvent replacement. This method is not suitable for commonly used organic solvents such as methanol and ethanol. Industrial-scale production can easily cause the solvent temperature to rise rapidly, posing a great safety hazard. Summary of the invention

[0005] The invention provides a method for preparing an aerogel composite material and an aerogel composite material. A supercritical high-pressure reactor is used as a container, wet gel and an alcohol solvent are mixed, and then heated and pressurized for solvent replacement. After the replacement is completed, supercritical drying is directly performed. The aerogel material prepared by the method maintains a complete skeleton structure, greatly reduces the amount of solvent used, shortens the solvent replacement cycle, is suitable for industrial-scale production, and solves the technical problems in the method for preparing the aerogel composite material, such as high cost and long process time of solvent replacement and supercritical drying, which seriously restricts production capacity.

[0006] According to one aspect of the present invention, a method for preparing an aerogel composite material is provided, comprising the following steps: S100, loading a wet gel into a supercritical high-pressure reactor, and performing solvent replacement in the supercritical high-pressure reactor, and utilizing the solvent replacement process to verify the airtightness of the supercritical high-pressure reactor; S200, performing supercritical drying directly in the supercritical high-pressure reactor.

[0007] Furthermore, the solvent replacement process is repeated 2 times or more.

[0008] Further, step S100 specifically includes: S101, loading the wet gel into a supercritical high-pressure reactor and keeping it airtight; S102, conveying the solvent into the supercritical high-pressure reactor, heating the supercritical high-pressure reactor and filling it with nitrogen until the preset temperature and pressure are reached, and maintaining a constant temperature and pressure state for ≥4h, standing, and replacing the water and reaction impurities in the wet gel; S103, stopping heating the supercritical high-pressure reactor and cooling it to below the boiling point of the solvent, releasing the gas, and discharging the solvent; S104, repeating S101 to S103, and repeating 2 to 5 times. Preferably, S102, maintaining a constant temperature and pressure state for 8 to 14h. If the time is too short, the water and impurity components in the solvent and wet gel will not diffuse sufficiently, and the replacement effect will not be obvious. 8 to 14h can achieve a better replacement effect. Further extending the time will have a limited improvement in the replacement rate but will extend the replacement cycle.

[0009] Furthermore, in step S102, the solvent in the solvent storage tank is transported to the supercritical high-pressure reactor, and the solvent level is kept higher than the aerogel and composite material in the wet gel. If the solvent does not completely cover the aerogel and composite material, the wet gel exposed above the solvent and the internal water of the composite material will not be fully replaced, and the exposed wet gel will easily evaporate and dry under heating conditions, resulting in cracking and collapse of the material.

[0010] Furthermore, the preset temperature in step S102 is higher than 40° C. When the temperature is too low, the diffusion rate between the solvent component and the impurity component is significantly reduced, and the replacement cycle to achieve the same replacement effect is significantly increased.

[0011] Further, the preset temperature is a temperature above the boiling point of the replacement solution and below the critical temperature. Further, the preset temperature is 50°C to 150°C. Further, under the conditions of heating and pressurization (close to or reaching a subcritical state), the compatibility and diffusion rate of the solvent are greatly improved, and if the temperature is too high, the energy consumption is higher and the danger is higher.

[0012] Furthermore, the preset pressure in step S102 is higher than 1.5 MPa.

[0013] Furthermore, the preset pressure is a pressure below the critical point of the solvent. Furthermore, the preset pressure in step S102 is 2-8 MPa. If the pressure is too low, the effect of increasing the displacement rate is not obvious, and if the pressure is too high, the safety risk increases.

[0014] Furthermore, the solvent used in the solvent replacement is a supercritical drying solvent, and the critical drying solvent is one of methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, and tert-butanol; the mass of the added solvent is 2 times or more of the wet gel. Preferably, the mass of the added solvent is 2 to 3 times the mass of the wet gel. Too little solvent cannot completely cover the product, and the replacement efficiency will be reduced. In order to keep the kettle volume not higher than the maximum allowable value, the higher the proportion of solvent added, the less wet gel is loaded into the kettle, the overall replacement efficiency is reduced, and the increased amount of solvent leads to increased costs.

[0015] According to another aspect of the present invention, an aerogel composite material is also provided, which is prepared by the preparation method of the aerogel composite material.

[0016] The present invention has the following beneficial effects:

[0017] The preparation method of the aerogel composite material of the present invention adopts a supercritical high-pressure reactor as a carrier for solvent replacement, places a wet gel in the supercritical high-pressure reactor and heats and pressurizes the reactor to improve the solvent replacement efficiency, the heating and pressurizing greatly improve the diffusion rate and compatibility of the solvent, accelerates the diffusion of water and other reaction impurities in the wet gel, greatly reduces the replacement time, and thus shortens the preparation cycle of the aerogel and the composite material thereof, and can shorten the replacement cycle from 5 to 10 days to less than 3 days, greatly saving the production cost, facilitating large-scale production, having a good replacement effect, and the prepared aerogel and the composite material thereof have a complete structure and stable performance; and the maximum pressure and The temperature is significantly higher than the temperature and pressure values ​​of the replacement process of the present invention, and the heating and pressurizing process to improve the efficiency of solvent replacement is carried out in a supercritical high-pressure reactor, which can effectively ensure the safety of the dissolution replacement process and the heating and pressurizing process; since the solvent replacement is carried out by heating and pressurizing, the solvent replacement process is also the airtightness verification process of the supercritical high-pressure reactor, and the duration of the heating and pressurizing used in the solvent replacement is far longer than the time required by the airtightness verification process, so it can completely replace the airtightness verification process, and the verification standard is higher than the existing airtightness verification requirements and standards; when the solvent replacement of the wet gel is completed, supercritical drying can be directly carried out in the supercritical high-pressure reactor. The characteristics of the supercritical high-pressure reactor, the solvent replacement and supercritical drying processes for the preparation of aerogel composite materials are fully matched and combined, and the supercritical high-pressure reactor can be effectively utilized, the utilization rate of the supercritical high-pressure reactor is improved, and the equipment cost is saved; it not only ensures that the safety of the solvent replacement is improved by heating and pressurizing the solvent replacement, but also saves the process of verifying the airtightness in the supercritical drying process, thereby shortening the preparation time of the entire aerogel composite material and saving production costs.

[0018] In addition to the above-described objects, features and advantages, the present invention has other objects, features and advantages. The present invention is further described in detail below. DETAILED DESCRIPTION

[0019] The following examples of the present invention are described in detail, but the present invention can be implemented in a variety of different ways as defined and covered below. Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0020] The preparation method of the aerogel composite material of this embodiment includes the following steps: S100, loading the wet gel into a supercritical high-pressure reactor, and performing solvent replacement in the supercritical high-pressure reactor, and using the solvent replacement process to verify the airtightness of the supercritical high-pressure reactor; S200, directly performing supercritical drying in the supercritical high-pressure reactor. The preparation method of the aerogel composite material of the present invention uses a supercritical high-pressure reactor as a carrier for solvent replacement, places the wet gel in the supercritical high-pressure reactor and heats and pressurizes to improve the efficiency of solvent replacement. Heating and pressurizing greatly improve the diffusion rate and compatibility of the solvent, accelerate the diffusion of water and other reaction impurities in the wet gel, and greatly reduce the replacement time, thereby shortening the preparation cycle of aerogel and its composite materials, and can shorten the replacement cycle from 5 to 10 days to less than 3 days, greatly saving production costs, facilitating large-scale production, and having good replacement effects. The prepared aerogel and its composite materials have complete structures and stable performances; and the maximum pressure and The temperature is significantly higher than the temperature and pressure values ​​of the replacement process of the present invention, and the heating and pressurizing process to improve the efficiency of solvent replacement is carried out in a supercritical high-pressure reactor, which can effectively ensure the safety of the dissolution replacement process and the heating and pressurizing process; since the solvent replacement is carried out by heating and pressurizing, the solvent replacement process is also the airtightness verification process of the supercritical high-pressure reactor, and the duration of the heating and pressurizing used in the solvent replacement is far longer than the time required by the airtightness verification process, so it can completely replace the airtightness verification process, and the verification standard is higher than the existing airtightness verification requirements and standards; when the solvent replacement of the wet gel is completed, supercritical drying can be directly carried out in the supercritical high-pressure reactor. The characteristics of the supercritical high-pressure reactor, the solvent replacement and supercritical drying processes for the preparation of aerogel composite materials are fully matched and combined, and the supercritical high-pressure reactor can be effectively utilized, the utilization rate of the supercritical high-pressure reactor is improved, and the equipment cost is saved; it not only ensures that the safety of the solvent replacement is improved by heating and pressurizing the solvent replacement, but also saves the process of verifying the airtightness in the supercritical drying process, thereby shortening the preparation time of the entire aerogel composite material and saving production costs.

[0021] In this embodiment, the solvent replacement process is repeated 2 times or more. If the number of solvent replacements is too small, the water in the wet gel cannot be effectively replaced; if the number of solvent replacements is too large, the improvement of the solvent replacement rate is limited, but it causes waste of solvent and energy, and the replacement cycle is also extended accordingly. Preferably, the solvent replacement process is repeated 2 to 5 times. The number of repeated solvent replacements is usually determined according to the characteristics and preparation conditions of the required aerogel. Repeating the solvent replacement 2 to 5 times can ensure that the water and other reaction impurities in the gel are fully replaced, thereby obtaining an aerogel with a good pore structure and low drying shrinkage; if the number of solvent replacements is less than 2 times, the original solvent may not be completely replaced, which may increase the shrinkage of the aerogel during the drying process, reduce its porosity and specific surface area, thereby affecting the final performance of the aerogel, and may even cause the product to be scrapped; and if the number of solvent replacements is more than 5 times, the improvement of the solvent replacement rate is limited, but it causes waste of solvent and energy, and the replacement cycle is also extended accordingly, which may bring some unnecessary costs and time consumption, and excessive solvent replacement may cause excessive expansion of the gel structure, affecting its stability and mechanical strength. In addition, excessive solvent replacement may also increase solvent consumption and disposal costs, as well as possible environmental impacts.

[0022] In this embodiment, step S100 specifically includes: S101, loading the wet gel into a supercritical high-pressure reactor and keeping it airtight; S102, conveying a solvent into the supercritical high-pressure reactor, heating the supercritical high-pressure reactor and filling it with nitrogen until a preset temperature and pressure are reached, and maintaining a constant temperature and pressure state for ≥4h, standing to replace water and reaction impurities in the wet gel; S103, stopping heating the supercritical high-pressure reactor and cooling it to below the boiling point of the solvent, releasing gas, and discharging the solvent; S104, repeating S101 to S103, and repeating 2 to 5 times. The wet gel is loaded into a supercritical high-pressure reactor and kept sealed. This step ensures the control of the internal environment of the reactor and provides a closed and controlled environment for the subsequent solvent replacement and drying process; the solvent is transported into the supercritical high-pressure reactor, heated and filled with nitrogen to the preset temperature and pressure, and maintained at a constant temperature and pressure state for ≥8 hours. This step is the most critical part of the whole process. The delivery of the solvent helps the water and reaction impurities in the wet gel to be effectively replaced; the solvent in the subcritical state has better solubility and diffusion ability than the liquid in the normal state, and can penetrate into the pores of the gel more evenly and thoroughly, thereby more effectively removing the water and impurities in the gel. Under the constant temperature and pressure state, the solvent can penetrate into every part of the gel more evenly, which helps to replace the water and impurities more thoroughly and ensure uniform replacement; long-term constant temperature and pressure treatment helps to reduce the shrinkage of the gel during the drying process and maintain its pore structure, which is crucial to maintaining the low density and high specific surface area characteristics of the aerogel; long-term treatment helps to form a more uniform pore structure, thereby obtaining a higher porosity. If the constant temperature and pressure state is maintained for less than 8 hours, or even less than 4 hours, insufficient time may result in the solvent failing to fully penetrate all parts of the gel, thereby failing to completely remove moisture and impurities; if the constant temperature and pressure are maintained for insufficient time, the gel may shrink unevenly during the drying process, resulting in damage to the pore structure and affecting the performance of the aerogel; insufficient treatment may increase the density of the aerogel, losing its advantage as a lightweight material; due to changes in pore structure and density, the thermal insulation performance, acoustic performance and mechanical properties of the aerogel may be affected, resulting in a decrease in overall performance. Preferably, S102, transporting the solvent into the supercritical high-pressure reactor, heating and filling the supercritical high-pressure reactor with nitrogen until the preset temperature and pressure are reached, and maintaining the constant temperature and pressure state for 8 to 14 hours, can achieve a better replacement effect, further extending the time of maintaining the constant temperature and pressure state, exceeding 14 hours, the improvement of the replacement rate is limited and it is easy to lead to an extension of the replacement cycle; the time of maintaining the constant temperature and pressure state is too short, less than 8 hours, or even less than 4 hours, the water and impurity components in the solvent and wet gel are not fully diffused, and the replacement effect is not obvious.S103, stop heating the supercritical high-pressure reactor and cool it down to below the boiling point of the solvent; after each heating replacement is completed, the temperature in the supercritical high-pressure reactor should be lowered to below the boiling point of the solvent before releasing the solvent, otherwise the solvent replacement process will become a drying process.

[0023] In this embodiment, in step S102, the solvent in the solvent storage tank is transported to the supercritical high-pressure reactor, and the solvent level is kept higher than the aerogel and composite materials in the wet gel. Ensuring that the solvent can fully contact the aerogel and composite materials in the wet gel helps the solvent to evenly penetrate into the pores of the gel, thereby more effectively replacing the water and reaction impurities in the gel; keeping the solvent level higher than the wet gel can reduce the possibility of local drying, which may cause uneven shrinkage of the aerogel structure and affect its pore structure and mechanical strength; maintaining the solvent level helps to maintain the wet state of the wet gel, which is crucial to maintaining the integrity of the gel structure and preventing defects caused by early drying; by controlling the solvent level, the solvent replacement rate and drying process can be adjusted, which helps to control the entire drying process and avoid structural damage caused by rapid drying. If the solvent level is lower than the aerogel and composite materials in the wet gel, insufficient solvent level may result in the inability to completely replace the moisture and other reaction impurities in the wet gel, affecting the purity and performance of the aerogel; too low a solvent level may cause local areas of the wet gel to contact the air prematurely, resulting in uneven drying, which may cause the collapse of the aerogel structure and changes in porosity; if the solvent level is too low, the wet gel may begin to dry without sufficient solvent replacement, which may damage the pore structure of the aerogel and reduce its mechanical strength; insufficient solvent level may cause cracks or other defects to form in the aerogel during the drying process, which will reduce the overall performance and application value of the aerogel; too low a solvent level may reduce the efficiency of the solvent replacement and drying process, extend the preparation time, and increase production costs.

[0024] In this embodiment, the preset temperature in step S102 is higher than 40°C. If the temperature is too low, the diffusion rate between the solvent component and the impurity component is significantly reduced, and the replacement cycle to achieve the same replacement effect is significantly increased. Preferably, the preset temperature in step S102 is 50°C to 150°C. Preferably, the preset temperature in step S102 is 50°C to 150°C. In this temperature range, the solvent can reach its subcritical state; subcritical fluids have unique solubility and diffusivity, and can more effectively penetrate into the pores of the gel, which helps to remove moisture and impurities; in the temperature range of 50°C to 150°C, the gel structure can be avoided from being destroyed due to excessive temperature, while promoting the penetration and exchange of the solvent, which helps to maintain the pore structure and mechanical integrity of the aerogel; and combined with maintaining a constant temperature and pressure state for ≥8 hours, it helps to improve the efficiency of solvent replacement and ensure that the moisture and impurities in the wet gel are completely removed; this temperature range is lower than the supercritical temperature of the solvent, which helps to ensure the safety of the operation and reduce energy consumption. When the preset temperature is too low and is lower than 50°C, or even lower than 40°C, the low temperature may cause the solvent to fail to reach a subcritical state, thereby affecting its solubility and diffusivity and reducing the efficiency of solvent replacement; the lower temperature may not be sufficient to promote the effective exchange of water and impurities between the solvent and the wet gel, resulting in incomplete replacement; the penetration rate of the solvent may slow down at low temperatures, and it will take longer to complete the replacement process, thereby extending the entire preparation cycle. When the preset temperature is too high and is higher than 150°C, the high temperature may cause thermal decomposition of certain components in the solvent or gel, affecting the chemical composition and properties of the aerogel; excessively high temperatures may cause the pore structure of the aerogel to collapse during the drying process, reducing its porosity and specific surface area; high-temperature operation may increase safety risks, such as accidental evaporation of the solvent or a sharp increase in the pressure inside the reactor; increasing the temperature will increase the energy consumption of the entire preparation process, thereby increasing production costs.

[0025] In this embodiment, the preset temperature is a temperature above the boiling point of the replacement solution and below the critical temperature. This temperature range helps the solvent to penetrate into the pores of the wet gel more effectively, thereby helping to replace the water and reaction impurities in the gel; keeping it below the supercritical temperature can ensure that the solvent remains in a liquid state and avoid direct drying of the material, which is necessary for the solvent replacement process; this temperature range is usually lower than the thermal decomposition temperature of the solvent or gel precursor, which helps to avoid decomposition of the material at high temperatures; under conditions above the boiling point but below the supercritical temperature, the solvent can approach its subcritical state, which helps to achieve solvent replacement in subsequent steps; the appropriate temperature helps to improve the efficiency of solvent replacement, ensure that the water and impurities in the wet gel are completely removed, and reduce shrinkage and structural damage during the drying process. When this temperature range is exceeded, the following may occur: If the temperature exceeds the supercritical temperature of the solvent, the solvent may form a supercritical state, resulting in the separation of the solvent and the gel, affecting the effect of solvent replacement; If the temperature is too high, certain components of the solvent or gel may undergo thermal decomposition, affecting the chemical composition and properties of the aerogel; Too high a temperature may cause the pore structure of the aerogel to collapse during the drying process, reducing its porosity and specific surface area; High-temperature operation may increase safety risks, such as accidental evaporation of the solvent or a sharp increase in the pressure inside the reactor; If the temperature is lower than the boiling point of the mixed solution, the solvent may not be able to reach the required liquid condition, thus affecting the solvent replacement process; Too low a temperature may slow down the penetration of the solvent, requiring longer time to complete the replacement process, thereby extending the entire preparation cycle.

[0026] In this embodiment, the preset pressure in step S102 is higher than 1.5MPa. Preferably, the preset pressure in step S102 is 1.5MPa to 7MPa. Preferably, the preset pressure in step S102 is 2MPa to 5MPa. If the pressure is too low, the effect of improving the replacement rate is not obvious, and if the pressure is too high, the safety risk increases. This pressure range generally covers the pressure required for certain solvents (such as methanol and ethanol) to reach their subcritical state. In the subcritical state, the solvent has unique solubility and diffusivity, which helps to efficiently replace water and impurities in the wet gel; it can prevent the solvent from evaporating or decomposing at high temperatures, ensuring that the solvent remains stable throughout the replacement process; appropriate pressure helps to maintain the stability of the aerogel pore structure and avoid the collapse of the pore structure during solvent replacement and drying; maintaining a constant pressure within this pressure range helps the solvent to diffuse evenly in the wet gel and achieve a more thorough replacement; this pressure range is generally considered to be a safe operating window, which can avoid equipment damage or safety accidents caused by excessive pressure. When the preset pressure is too low and below 1.5MPa, the solvent may not reach the subcritical state, which will affect its solubility and diffusivity and reduce the replacement efficiency; under lower pressure, the solvent is more likely to volatilize, which may lead to solvent loss and environmental problems; insufficient pressure may prevent the solvent from fully penetrating into the pores of the wet gel, making it impossible to completely remove moisture and impurities. When the preset pressure is too high and above 7MPa, the excessive pressure requires the use of higher standard equipment and materials, increasing costs; as the pressure increases, the safety risks of equipment and operations also increase, and stricter safety measures may be required; excessive pressure may cause the decomposition of certain components in the solvent or gel, affecting the quality and performance of the aerogel; extreme pressure conditions may cause the destruction of the aerogel pore structure, reducing its specific surface area and porosity.

[0027] In this embodiment, the preset pressure is the pressure below the critical point of the solvent. Within this pressure range, the density and permeability of the solvent increase, which helps to penetrate deeper into the pores of the wet gel, thereby more effectively replacing the water and impurities therein; appropriate pressure helps to maintain the three-dimensional network structure of the wet gel during the solvent replacement process and avoid collapse during the drying process; pressure above the subcritical pressure helps to enhance the interaction between the solvent and the gel and improve the efficiency of solvent replacement; this pressure range is prepared for supercritical drying, and when the pressure and temperature reach the supercritical point at the same time, a more gentle and uniform drying process can be achieved; staying above the subcritical pressure can slow down the evaporation of the solvent and help maintain the solvent concentration in the reactor. When the pressure range is exceeded (there is no upper limit pressure in the supercritical state), higher standard equipment may be required to withstand higher pressures, which will increase costs. Higher pressures may increase safety risks in operations, including the possibility of equipment failure and leakage. Extreme pressure conditions may cause decomposition of certain components in the solvent or gel, affecting the quality and performance of the aerogel; below the subcritical pressure: too low pressure may lead to reduced permeability and replacement efficiency of the solvent, and failure to completely remove moisture and impurities in the wet gel. Too low pressure may result in uneven drying process, affecting the pore structure and mechanical properties of the aerogel. Solvents are more likely to evaporate at lower pressures, which may lead to solvent loss and environmental problems.

[0028] In this embodiment, the solvent used in the solvent replacement is a supercritical drying solvent, and the supercritical drying solvent is one of methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, and tert-butanol; the mass of the added solvent is 2 times or more of the wet gel. Preferably, the mass of the added solvent is 2 to 3 times the mass of the wet gel. Too little solvent cannot completely cover the product, and the replacement efficiency will be reduced; in order to keep the kettle volume not higher than the maximum allowed, the higher the proportion of solvent added, the less wet gel is loaded in the kettle, the overall replacement efficiency is reduced, and the increase in solvent consumption leads to increased costs. Commonly used supercritical drying solvents such as methanol and ethanol are selected for replacement. Such solvents are non-toxic or low-toxic, and are cheap. At the same time, it is ensured that the product can be directly supercritically dried after replacement, and the process is simple and convenient.

[0029] The aerogel composite material of this embodiment is prepared by using the above-mentioned preparation method of the aerogel composite material.

[0030] During implementation, a highly efficient replacement and drying method for aerogel and its composite materials is provided. The method uses a supercritical high-pressure reactor as a container, mixes wet gel and alcohol solvent, heats and pressurizes them for solvent replacement, and directly performs supercritical drying after the replacement is completed. The aerogel material prepared by this method maintains a complete skeleton structure, greatly shortens the solvent replacement cycle, and is suitable for industrial-scale production. The method includes the following steps:

[0031] S1. Load the wet gel into a supercritical high-pressure reactor and put down the reactor cover to keep it airtight;

[0032] S2, transporting the solvent in the solvent storage tank to the supercritical high-pressure reactor, and keeping the solvent liquid level higher than the aerogel and the composite material;

[0033] S3, heating to keep the temperature in the reactor stable, and filling with nitrogen to keep the pressure in the reactor stable;

[0034] S4, maintaining a constant temperature and pressure state in the kettle for ≥ 8 hours, allowing it to stand to displace water and other reaction impurities in the wet gel;

[0035] S5, stop heating, open the vent valve, and release the gas in the reactor;

[0036] S6, discharging the solvent through the drain port;

[0037] S7, repeat S2 to S5 process 2 to 5 times;

[0038] S8. Supercritical drying.

[0039] The method of the present invention uses a supercritical high-pressure reactor as a displacement container. In order to ensure the safety of the supercritical drying process, the supercritical drying process needs to be pre-filled with gas before supercritical drying to maintain pressure to verify the air tightness of the kettle body. This process takes a long time (more than 8 hours); the solvent replacement process is carried out for a long time to maintain heat and pressure to verify the air tightness of the kettle body. Direct supercritical drying after solvent replacement can save the process of verifying air tightness, reducing the supercritical drying time. Pressurizing the solvent replacement under heating conditions can greatly improve the replacement efficiency and shorten the time of static replacement. It is believed that this is because by controlling the temperature and pressure in the replacement container, it is in a subcritical fluid state or close to a subcritical fluid state, and the diffusion rate and compatibility of the subcritical fluid are greatly improved.

[0040] Furthermore, the solvent added in the above step S2 is one of the solvents for supercritical drying such as methanol, ethanol, isopropanol, etc., and the mass of the added solvent is 2 to 3 times that of the aerogel.

[0041] Furthermore, in the above step S3, the temperature in the reactor is kept stable at 50-150° C., and further, the temperature is preferably kept above the boiling point and below the supercritical temperature.

[0042] Furthermore, in the above step S3, the pressure in the reactor is kept stable at 1.5-7 MPa. Furthermore, the pressure is preferably kept above the subcritical pressure and below the supercritical pressure.

[0043] According to the method of the present invention, aerogel and composite materials thereof are prepared, and the supercritical high-pressure reactor is used as a displacement container, which can effectively utilize the equipment, improve the utilization rate of the equipment, and save equipment costs. The process of verifying airtightness in the supercritical drying process is omitted, the time of the supercritical drying process is shortened, and production costs are saved. The maximum pressure and temperature that the supercritical high-pressure reactor can withstand are significantly higher than the temperature and pressure values ​​of the displacement process of the present invention, ensuring the safety of the displacement process.

[0044] Commonly used supercritical drying solvents such as methanol and ethanol are selected for replacement. Such solvents are non-toxic or low-toxic and inexpensive. At the same time, they ensure that the product can be directly supercritically dried after replacement, and the process is simple and convenient.

[0045] Heating and pressurizing greatly improve the diffusion rate and compatibility of the solvent, accelerate the diffusion of water and other reaction impurities in the wet gel, and greatly reduce the replacement time, thereby shortening the preparation cycle of aerogels and their composite materials from 8 to 10 days to less than 3 days, greatly saving production costs and facilitating large-scale production. The replacement effect is good, and the prepared aerogels and their composite materials have complete structures and stable performance.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] (1) The method of the present invention improves the replacement efficiency, shortens the preparation cycle, and saves production costs.

[0048] (2) The process of the method of the present invention is simple, convenient, safe and reliable.

[0049] (3) The method of the present invention improves the utilization rate of equipment, saves equipment cost, and the prepared products are stable and reliable.

[0050] Embodiment 1:

[0051] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0052] Embodiment 2:

[0053] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 1.5MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0054] Embodiment 3:

[0055] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 7MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0056] Embodiment 4:

[0057] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 40℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0058] Embodiment 5:

[0059] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 100℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0060] Embodiment 6:

[0061] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 12kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0062] Embodiment 7:

[0063] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 12h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0064] Embodiment 8:

[0065] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 4h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0066] Embodiment 9:

[0067] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 5 times and then perform supercritical drying.

[0068] Embodiment 10:

[0069] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 8kg of ethanol into the reactor, keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0070] Comparative Example 1:

[0071] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 25℃, do not fill with nitrogen, open the pressure relief valve, and control the pressure to normal pressure; keep the reactor at a constant temperature and pressure state for 24h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 7 times and then perform supercritical drying.

[0072] Comparative Example 2:

[0073] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, do not fill with nitrogen, open the pressure relief valve, and control the pressure to normal pressure; keep the reactor at a constant temperature and pressure state for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0074] Comparative Example 3:

[0075] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 25℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0076] Comparative Example 4:

[0077] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 1MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0078] Comparative Example 5:

[0079] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 280℃, then fill it with nitrogen to keep the pressure stable at 10MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0080] Comparative Example 6:

[0081] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 2h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0082] Comparative Example 7:

[0083] Place the wet gel composite material A with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 4kg of ethanol into the reactor, keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement 3 times and then perform supercritical drying.

[0084] Comparative Example 8:

[0085] Place the A wet gel composite material with a mass of 4kg and a water content of 50wt% in a 50L supercritical high-pressure reactor, put down the reactor cover, and tighten it to keep it airtight; transport 10kg of ethanol into the reactor, and keep the ethanol liquid level 60mm higher than the composite material; heat the reactor to keep the temperature stable at 70℃, then fill it with nitrogen to keep the pressure stable at 4MPa; keep the reactor at a constant temperature and pressure for 8h; stop heating, open the vent valve, and slowly release the gas in the reactor; discharge the ethanol in the reactor through the drain port. Repeat the replacement once and then perform supercritical drying.

[0086] The aerogel composite materials obtained by the above examples and comparative examples, and the preparation process parameters of the aerogel composite materials are shown in Table 1.

[0087] Table 1 Preparation process parameters of aerogel composites

[0088] / Pressure / MPa Temperature / ℃ Mass multiple / times Time / h Replacement quantity / times Example 1 4 70 2.5 8 3 Example 2 1.5 70 2.5 8 3 Example 3 7 70 2.5 8 3 Example 4 4 40 2.5 8 3 Example 5 4 100 2.5 8 3 Example 6 4 70 3 8 3 Example 7 4 70 2.5 12 3 Example 8 4 70 2.5 4 3 Example 9 4 70 2.5 8 5 Example 10 4 70 2 8 3 Comparative Example 1 Normal pressure 25 2.5 24 7 Comparative Example 2 Normal pressure 70 2.5 8 3 Comparative Example 3 4 25 2.5 8 3 Comparative Example 4 1 70 2.5 8 3 Comparative Example 5 10 280 2.5 8 3 Comparative Example 6 4 70 2.5 2 3 Comparative Example 7 4 70 1.0 8 3 Comparative Example 8 4 70 2.5 8 1

[0089] As shown in Table 2, the concentration of ethanol after each replacement of each replacement scheme and the obtained aerogel composite material are compared.

[0090] Table 2 Aerogel composites

[0091]

[0092] Conclusion 1: Comparing Example 1 with Example 2, the pressure of high temperature and high pressure is reduced from 4 MPa to 1.5 MPa, the solvent is replaced, the first replacement rate is increased, the second and third replacement rates are reduced, and the quality of the aerogel composite material obtained after supercritical drying is reduced.

[0093] Conclusion 2: Comparing Example 1 with Example 3, the pressure of high temperature and high pressure increased from 4 MPa to 7 MPa, the first, second and third replacement rates increased, the total time increased (increased by 4 h), and the quality of the aerogel composite materials obtained after supercritical drying was intact.

[0094] Conclusion 3: Comparing Example 1 with Example 4, the temperature of high temperature and high pressure was reduced from 70°C to 40°C, the solvent was replaced, the first replacement rate was increased, the second and third replacement rates were reduced, the total time was reduced (reduced by 2h), and the quality of the aerogel composite material obtained after supercritical drying was reduced.

[0095] Conclusion 4: Comparing Example 1 with Example 5, the temperature of high temperature and high pressure was increased from 70°C to 100°C, the solvent was replaced, the first replacement rate decreased, the second and third replacement rates increased, the total time increased (increased by 2h), and the quality of the aerogel composite materials obtained after supercritical drying was intact.

[0096] Conclusion 5: Comparing Example 1 with Example 6, the mass of added solvent increased (increased by 0.5 times), the solvent replacement, the first, second and third replacement rates were all improved, and the quality of the aerogel composite material obtained after supercritical drying was intact.

[0097] Conclusion 6: Compared with Example 1 and Example 7, the time for maintaining the constant temperature and pressure state is extended from 8 h to 12 h, the solvent is replaced, the first replacement rate is reduced, the second and third replacement rates are increased, the total time is increased (increased by 12 h), and the quality of the aerogel composite materials obtained after supercritical drying is intact.

[0098] Conclusion 7: Compared with Example 1 and Example 8, the time for maintaining the constant temperature and pressure state is reduced from 8 h to 4 h, the solvent is replaced, the first and second replacement rates are improved, the third replacement rate is reduced, the total time is reduced (reduced by 12 h), and the quality of the aerogel composite material obtained after supercritical drying is reduced.

[0099] Conclusion 8: Comparing Example 1 with Example 9, the number of solvent replacements increased from 3 to 5 times, and the solvent replacement rates from the first to the fifth times gradually increased, and the fifth replacement rate reached 98.2%. The total time increased (increased by 16 hours), and the quality of the aerogel composite materials obtained after supercritical drying was intact.

[0100] Conclusion 9: Comparing Example 1 with Example 10, the mass of added solvent is reduced (reduced by 0.5 times), the solvent replacement, the first, second and third replacement rates are all reduced, and the quality of the aerogel composite material obtained after supercritical drying is reduced.

[0101] Conclusion 10: In comparative example 1, the aerogel composite material was prepared by the conventional method, and the solvent was replaced 7 times, with a total time of 180 h. Although the quality of the obtained aerogel composite material was intact, it was time-consuming and seriously restricted the production capacity.

[0102] Conclusion 11: Comparing Example 1 with Comparative Example 2, the pressure of high temperature and high pressure was reduced from 4 MPa to normal pressure, the solvent was replaced, the first replacement rate was significantly improved, the second replacement rate was slightly improved, the third replacement rate was significantly reduced, the total time was reduced (reduced by 2 hours), and the aerogel composite product obtained after supercritical drying had cracking phenomenon, that is, the product was unqualified.

[0103] Conclusion 12: Comparing Example 1 with Comparative Example 3, the temperature of high temperature and high pressure was reduced from 70°C to 25°C, the solvent was replaced, the first replacement rate was significantly improved, the second replacement rate was slightly improved, the third replacement rate was significantly reduced, the total time was reduced (reduced by 2h), and the aerogel composite product obtained after supercritical drying had cracking, that is, the product was unqualified.

[0104] Conclusion 13: Comparing Example 1 with Comparative Example 4, the pressure of high temperature and high pressure was reduced from 4 MPa to 1 MPa, the solvent was replaced, the first replacement rate was significantly improved, the second replacement rate was reduced, the third replacement rate was significantly reduced, the total time was reduced (reduced by 1 h), and the aerogel composite product obtained after supercritical drying had cracking, that is, the product was unqualified.

[0105] Conclusion 14: When Example 1 is compared with Comparative Example 5, the pressure of high temperature and high pressure is increased from 4 MPa to 10 MPa, and the temperature is increased from 70°C to 280°C. The first replacement product already has cracking, that is, the product is unqualified.

[0106] Conclusion 15: Comparing Example 1 with Comparative Example 6, the time for maintaining the constant temperature and pressure state is reduced from 8 hours to 2 hours, the solvent is replaced, the first replacement rate is significantly improved, the second replacement rate is significantly reduced, the third replacement rate is significantly reduced, the total time consumption is reduced (reduced by 18 hours), and the aerogel composite product obtained after supercritical drying has cracking phenomenon, that is, the product is unqualified.

[0107] Conclusion 16: When Example 1 is compared with Comparative Example 7, the mass of added solvent is reduced (reduced by 1.5 times), the solvent replacement, and the first, second, and third replacement rates are all significantly reduced. The aerogel composite product obtained after supercritical drying has top cracking, that is, the product is unqualified.

[0108] Conclusion 17: Comparing Example 1 with Comparative Example 8, the number of solvent replacements was reduced from 3 times to 1 time, and the first replacement rate of solvent replacement was close, while the second and third replacements were missing. The total time consumption was reduced (reduced by 16 hours), and the aerogel composite product obtained after supercritical drying had cracking, that is, the product was unqualified.

[0109] Matters not covered by the present invention are known technologies.

[0110] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0111] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

[0112] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an aerogel composite material, characterized in that: The following steps are involved: S100, loading the wet gel into a supercritical high-pressure reactor, and performing solvent replacement in the supercritical high-pressure reactor, and using the solvent replacement process to verify the air tightness of the supercritical high-pressure reactor; S200, supercritical drying is carried out directly in a supercritical high-pressure reactor.

2. The method for preparing an aerogel composite material according to claim 1, characterized in that: The solvent replacement process was repeated 2 or more times.

3. The method for preparing an aerogel composite material according to claim 2, characterized in that: Step S100 specifically includes: S101, placing the wet gel into a supercritical high-pressure reactor and keeping it airtight; S102, transporting a solvent into a supercritical high-pressure reactor, heating the supercritical high-pressure reactor and filling it with nitrogen until a preset temperature and pressure are reached, and maintaining a constant temperature and pressure state for ≥ 4 hours, and standing to displace water and reaction impurities in the wet gel; S103, stopping heating the supercritical high-pressure reactor and cooling it to below the boiling point of the solvent, releasing gas, and discharging the solvent; S104. Repeat S101 to S103 2 to 5 times.

4. The method for preparing an aerogel composite material according to claim 3, characterized in that: In step S102, the solvent in the solvent storage tank is transported to the supercritical high-pressure reactor, and the solvent liquid level is kept higher than the aerogel and composite material in the wet gel.

5. The method for preparing an aerogel composite material according to claim 3, characterized in that: The preset temperature in step S102 is higher than 40°C.

6. The method for preparing an aerogel composite material according to claim 5, characterized in that: The preset temperature is a temperature above the boiling point of the replacement solution and below the critical temperature.

7. The method for preparing an aerogel composite material according to claim 3, characterized in that: The preset pressure in step S102 is higher than 1.5 MPa.

8. The method for preparing an aerogel composite material according to claim 7, characterized in that: The preset pressure is a pressure below the critical point of the solvent.

9. The method for preparing an aerogel composite material according to any one of claims 1 to 8, characterized in that: The solvent used in the solvent replacement is a supercritical drying solvent, and the supercritical drying solvent is one of methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, and tert-butanol; The mass of the added solvent is 2 times or more of the wet gel.

10. An aerogel composite material, characterized in that: The aerogel composite material is prepared by the preparation method of any one of claims 1 to 9.

Citation Information

Cited By

  • Alcohol replacement container and method for aerogel and aerogel composite material

    CN121695787A