Preparation equipment and preparation method of polyacrylonitrile spinning solution
By using a microchannel reactor and a circulation reaction device in the preparation of polyacrylonitrile spinning stock solution, combined with the impact and shear force of the disk, the problem of insufficient micro-mixture and heat transfer performance in the stirred tank reactor is solved, and the problem of insufficient micro-mixture and heat transfer performance in the stirred tank reactor is achieved. The reduction of molecular weight distribution and the improvement of polymerization efficiency enhance safety and deseasoning and deseasoning efficiency.
Patent Information
- Application Number
- CN202411175571.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-01
AI Technical Summary
The micro-mixture and heat transfer properties of existing stirred tank reactors are limited, resulting in a wide molecular weight distribution of the polyacrylonitrile spinning stock solution, long polymerization time and safety hazards.
Using microchannel reactor and circulation reaction device, the heat transfer of the polymerization process is enhanced through low viscosity fast exothermic reaction in the microchannel and high viscosity ordinary exothermic reaction in the circulation reaction device. and micro-mixed properties.
The molecular weight distribution range of polyacrylonitrile is significantly reduced, the efficiency of polymerization reaction is improved, the equipment size is reduced, and safety and deseasoning and deseasoning efficiency are improved.
Smart Images

Figure CN118874366A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyacrylonitrile spinning solution preparation, and specifically relates to polyacrylonitrile spinning solution preparation equipment and a preparation method. Background Art
[0002] Polyacrylonitrile spinning solution is a product synthesized by using dimethyl sulfoxide as solvent to make the raw material acrylonitrile undergo free radical polymerization under the action of an initiator. The activation energy of the free radical polymerization process is low (20-34kJ / mol), and the reaction is a rapid exothermic reaction; while the activation energy of the initiator decomposition into free radicals is high (105-150kJ / mol), which is not a rapid reaction, and the degree of uniformity of free radical dispersion determines the quality of the polymerization effect. Therefore, the initiator decomposition and micro-mixing performance are the control steps of the polymerization process. In addition, the endothermic process of initiator decomposition and the exothermic process of free radical polymerization both need to ensure the high efficiency of heat transfer. In short, the micro-mixing performance and heat transfer performance of the reactor determine the efficiency of the reaction process and the molecular weight distribution of the polyacrylonitrile product.
[0003] At present, the existing industrial synthesis methods of polyacrylonitrile-based carbon fiber polymerization stock solutions are mainly based on stirred tank reactors. However, the micro-mixing performance and heat transfer performance of stirred tank reactors are limited, and the viscosity of the material gradually increases as the reaction proceeds, and the micro-mixing and heat transfer performance will further decrease. Therefore, the polyacrylonitrile spinning stock solution products synthesized by stirred tank reactors have the disadvantages of long polymerization time and wide molecular weight distribution; in addition, the polymerization tank has a large liquid holding capacity, and uneven polymerization stirring will also lead to local explosions, which poses a great safety hazard. Summary of the invention
[0004] Therefore, the present invention provides a polyacrylonitrile spinning solution preparation device and preparation method, which can solve the technical problem that the micro-mixing performance and heat transfer performance of the stirred tank reactor in the prior art are limited, resulting in a wide molecular weight distribution of the processed polyacrylonitrile spinning solution product.
[0005] In order to solve the above problems, the present invention provides a polyacrylonitrile spinning solution preparation device, which includes a microchannel reactor and a circulating reaction device, wherein the microchannel reactor includes a microchannel, an inlet arranged at one end of the microchannel, and an outlet arranged at the other end of the microchannel; the inlet includes an inlet for an initiator solution and an inlet for a polymerization raw material solution;
[0006] The circulation reaction device includes a first reaction container, a first disc, a first drainage tube and a first driving mechanism. The first disc is arranged in the first reaction container. The first driving mechanism is used to drive the first disc to rotate. The solution at the outlet can flow into the first drainage tube. The outlet of the first drainage tube is opposite to the disk surface of the first disc, so that the solution at the outlet of the first drainage tube can collide with the disk surface of the first disc.
[0007] In some embodiments, the polyacrylonitrile spinning solution preparation device further includes a polymerization buffer tank and a first pump body, and the solution in the first reaction container can flow into the polymerization buffer tank;
[0008] The first pump body is used to pump at least a portion of the solution in the polymerization buffer tank into the first drainage pipe.
[0009] In some embodiments, the polyacrylonitrile spinning solution preparation equipment further includes a stirring mechanism, and the stirring mechanism is used to stir the solution in the polymerization buffer tank.
[0010] In some embodiments, the polyacrylonitrile spinning solution preparation device further includes a single-removal device, the single-removal device includes a second reaction container, a second disc, a second drainage tube, a second driving mechanism and a first negative pressure mechanism, the first negative pressure mechanism is used to evacuate the interior of the second reaction container;
[0011] Among them, the second disc is arranged in the second reaction container, and the second driving mechanism is used to drive the second disc to rotate; the solution in the polymerization buffer tank can flow into the second drainage tube, and the outlet of the second drainage tube is opposite to the disk surface of the second disc, so that the solution at the outlet of the second drainage tube can collide with the disk surface of the second disc.
[0012] In some embodiments, the inlet of the second drainage pipe is communicated with the outlet of the first pump body, so that the solution in the polymerization buffer tank is pumped into the second drainage pipe through the first pump body.
[0013] In some embodiments, the polyacrylonitrile spinning solution preparation device further includes a degassing device, the degassing device includes a third reaction container, a third disc, a third drainage pipe, a third driving mechanism and a second negative pressure mechanism, and the second negative pressure mechanism is used to evacuate the interior of the third reaction container;
[0014] Among them, the third disc is arranged in the third reaction container, and the third driving mechanism is used to drive the third disc to rotate; the solution in the second reaction container can flow into the third drainage tube, and the outlet of the third drainage tube is opposite to the disk surface of the third disc, so that the solution at the outlet of the third drainage tube can collide with the disk surface of the third disc.
[0015] In some embodiments, the polyacrylonitrile spinning solution preparation equipment further includes a second pump body, and the solution in the second reaction container is pumped into the third drainage tube through the second pump body.
[0016] In some embodiments, the lower portion of the third reaction container tapers from top to bottom.
[0017] In some embodiments, the polyacrylonitrile spinning solution preparation device further includes a polymer raw material storage tank and a polymer raw material feeding pump, wherein the polymer raw material feeding pump is used to pump the polymer raw material solution in the polymer raw material storage tank to the polymer raw material solution inlet;
[0018] And / or, the polyacrylonitrile spinning solution preparation equipment also includes an initiator solution storage tank and an initiator solution feeding pump, and the initiator solution feeding pump is used to pump the initiator solution in the initiator solution storage tank to the initiator solution inlet.
[0019] The present invention also provides a method for preparing polyacrylonitrile spinning solution, which is used to use the polyacrylonitrile spinning solution preparation device described in any one of the above, and the preparation method comprises the following steps:
[0020] preparing a polymerization raw material solution and an initiator solution;
[0021] Introducing a polymerization raw material solution into the polymerization raw material solution inlet, and introducing the initiator solution into the initiator solution inlet; wherein the temperature of the polymerization raw material solution is higher than the temperature of the initiator solution;
[0022] The first driving mechanism drives the first disk to rotate, and the solution at the outlet flows into the first drainage tube. The solution at the outlet of the first drainage tube collides with the disk surface of the first disk.
[0023] In some embodiments, the rotation speed of the first disc is 400-2800 r / min;
[0024] And / or, the feed mass ratio of the polymerization raw material solution to the initiator solution at the microchannel is (4-6):1;
[0025] And / or, the average residence time of the polymerization feed solution and the initiator solution in the microchannel is 1-60 minutes.
[0026] In some embodiments, the preparation method further comprises: introducing the solution in the circulation reactor into the polymerization buffer tank, and the first pump body pumps the solution in the polymerization buffer tank into the first drainage pipe and the second drainage pipe respectively;
[0027] Wherein, the mass ratio of the solution pumped into the first drainage tube and the second drainage tube by the first pump body is (20-50):1; and / or, the average residence time of the solution at the outlet in the circulation reaction device is 10-120 minutes.
[0028] In some embodiments, the solution at the outlet of the second drainage tube collides with the disk surface of the second disk;
[0029] Wherein, the negative pressure in the second reaction container is 1-10 kPaa; and / or the rotation speed of the second disc is 400-2800 r / min.
[0030] In some embodiments, the preparation method further comprises: introducing the solution in the second reaction container into the third drainage tube, and the solution at the outlet of the third drainage tube collides with the disk surface of the third disk;
[0031] Wherein, the negative pressure in the third reaction container is 0.5-2 kPaa; and / or the rotation speed of the third disc is 400-2800 r / min.
[0032] In some embodiments, the polymerization raw material solution is prepared by mixing acrylonitrile, a second monomer and dimethyl sulfoxide;
[0033] and / or, the temperature of the polymerization raw material solution is 65-70° C.;
[0034] And / or, the initiator solution is prepared by mixing an initiator and dimethyl sulfoxide;
[0035] And / or, the temperature of the initiator solution is 22-28°C.
[0036] The polyacrylonitrile spinning solution preparation device and preparation method provided by the present invention have the following beneficial effects:
[0037] 1. Compared with the simple stirring processing method in the prior art, the present invention divides the polymerization process of the initiator solution and the polymerization raw material solution into a low-viscosity rapid exothermic reaction process in a microchannel reactor and a high-viscosity ordinary exothermic reaction process in a circulating reaction device. The combination of the two can enhance the heat transfer and micro-mixing performance of the polymerization process, thereby greatly narrowing the molecular weight distribution range of polyacrylonitrile, greatly improving the process efficiency of the polymerization reaction, and obtaining a preliminary polyacrylonitrile spinning stock solution with a narrow molecular weight distribution.
[0038] 2. Compared with the traditional packed tower, the polymer liquid in the second reaction vessel and the third reaction vessel can have a larger gas-liquid contact area by using discs for deaeration and degassing, which greatly improves the deaeration and degassing efficiency; it can also reduce the size of the equipment and greatly increase the feeding speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0040] Figure 1 It is a structural schematic diagram of the polyacrylonitrile spinning solution preparation equipment of the present invention.
[0041] The accompanying drawings are marked as follows:
[0042] 1. Polymerization raw material storage tank; 2. Initiator solution storage tank; 3. Microchannel reactor; 4. First reaction container; 5. Polymerization buffer tank; 6. Second reaction container; 7. Third reaction container; 8. First negative pressure mechanism; 9. Second negative pressure mechanism; 10. Initiator solution feeding pump; 11. Polymerization raw material feeding pump; 12. First pump body; 13. Second pump body; 14. Post-degassing polymerization liquid delivery pump; 21. Initiator solution inlet; 101. Polymerization raw material solution inlet; 31. Microchannel; 301. Outlet; 41. First drainage tube; 42. First disc; 43. First driving mechanism; 51. Stirring mechanism; 61. Second drainage tube; 62. Second driving mechanism; 63. Second disc; 71. Third drainage tube; 72. Third driving mechanism; 73. Third disc. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings. They are only for the convenience of describing the present invention and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the devices or elements referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of the present invention. The directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.
[0045] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0046] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0047] See also Figure 1 As shown, according to an embodiment of the present invention, a polyacrylonitrile spinning solution preparation device is provided, which includes a microchannel reactor 3 and a circulating reaction device. The microchannel reactor 3 includes a microchannel 31, an inlet arranged at one end of the microchannel 31, and an outlet 301 arranged at the other end of the microchannel 31. Among them, the inlet includes an initiator solution inlet 21 and a polymerization raw material solution inlet 101. Among them, the initiator solution inlet 21 and the polymerization raw material solution inlet 101 can be connected to one end of the microchannel 31 in a Y-shaped manner.
[0048] The aforementioned cyclic reaction device includes a first reaction container 4, a first disc 42, a first drainage tube 41 and a first driving mechanism 43. The first disc 42 is arranged in the first reaction container 4, and the first driving mechanism 43 is used to drive the first disc 42 to rotate. Preferably, the center line of the first disc 42 is arranged vertically, and the first disc 42 rotates around its center line. The first driving mechanism 43 includes a first motor to drive the first disc 42 to rotate by the first motor.
[0049] The solution at the outlet 301 can flow into the first drainage tube 41. In some embodiments, the outlet 301 can be located above the first drainage tube 41, and the solution at the outlet 301 can flow to the first drainage tube 41 under the action of gravity. Of course, the solution at the outlet 301 can also be pumped into the first drainage tube 41 by a pump body. The outlet of the first drainage tube 41 is opposite to the disk surface of the first disk 42, so that the solution at the outlet of the first drainage tube 41 can collide with the disk surface of the first disk 42.
[0050] The preparation principle of acrylonitrile spinning solution in the above example is explained below:
[0051] The microchannel reactor 3 and the circulating reaction device cooperate to divide the preparation process of acrylonitrile spinning solution into two stages. Specifically, the initiator solution flows into the microchannel 31 from the initiator solution inlet 21, and the polymerization raw material solution flows into the microchannel 31 from the polymerization raw material solution inlet 101. The initiator solution and the polymerization raw material solution both undergo a first-stage reaction in the microchannel 31, and the solution flowing out from the outlet 301 of the microchannel 31 enters the circulating reaction device for a second-stage circulating reaction. After the reaction is complete, a preliminary polyacrylonitrile spinning solution is obtained.
[0052] Among them, the reaction of the first stage starts at the contact point of the two-phase fluid of the microchannel reactor 3. The temperature of the initiator solution injected into the microchannel reactor 3 is generally about 25°C, and the temperature of the polymerization raw material solution is generally about 70°C. As the initiator solution and the polymerization raw material solution are injected into the microchannel 31 at the same time, the initiator solution gradually heats up and is evenly dissolved in the polymerization raw material solution. The reaction of the first stage is relatively violent. The first stage is a low-viscosity, fast exothermic reaction. The microchannel 31 can greatly increase the heat transfer area of the polymerization reaction process, ensure that the heat released by the reaction can be transferred to the low-temperature phase in time, so that the free radicals of the initiator are evenly dispersed in the polymerization raw material solution, thereby effectively reducing the molecular weight distribution range of polyacrylonitrile. In addition, the reaction of the first stage has no amplification effect, which is convenient for industrial application.
[0053] After the first stage of reaction, the solution viscosity of the outlet 301 of the microchannel 31 is relatively high, making the reaction in the circulation reaction device a high viscosity reaction. The solution of the outlet 301 of the microchannel 31 collides with the disk surface of the first disk 42, and the first disk 42 uses centrifugal force and shear force to disperse the polymerization solution into micron-level liquid film and droplets. The liquid achieves rapid microscopic mixing during the polymerization and dispersion process, so that the initiator, acrylonitrile and the second monomer can be evenly dispersed and then gradually undergo polymerization reaction, thereby enhancing the internal microscopic mixing performance and heat transfer performance of the solution, further narrowing the molecular weight distribution range of polyacrylonitrile, and obtaining a preliminary polyacrylonitrile spinning stock solution with a narrow molecular weight distribution.
[0054] In the above example, the reaction in the microchannel reactor 3 is a low-viscosity, fast exothermic reaction, and the reaction in the circulating reaction device is a high-viscosity, ordinary exothermic reaction. Compared with the simple stirring processing method in the prior art, the present invention divides the polymerization process of the initiator solution and the polymerization raw material solution into a low-viscosity, fast exothermic reaction process in the microchannel reactor 3 and a high-viscosity, ordinary exothermic reaction process in the circulating reaction device. The combination of the two can enhance the heat transfer and micro-mixing performance of the polymerization process, which can greatly narrow the molecular weight distribution range of polyacrylonitrile, greatly improve the process efficiency of the polymerization reaction, and obtain a preliminary polyacrylonitrile spinning stock solution with a narrow molecular weight distribution.
[0055] It should be noted here that: compared with the traditional stirred tank reactor, the heat transfer area provided by the aforementioned microchannel reactor 3 is increased by 2-3 orders of magnitude, so that the heat generated by the polymerization can be transferred to the low-temperature heat transfer medium in a timely manner, which is conducive to making the free radicals of the initiator evenly dispersed in the polymerization raw material solution. The setting of the above-mentioned circulating reaction device ensures that the product has a high yield.
[0056] The aforementioned microchannel reactor 3 cooperates with the circulating reaction device to reduce the polymerization time and the size of the equipment, improve the product quality and process efficiency of polyacrylonitrile, and enhance the safety of the production process.
[0057] In some embodiments, the outer diameter of the aforementioned microchannel 31 may be between 10-1000 μm, preferably, the outer diameter of the microchannel 31 is 500-1000 μm. The length of the microchannel 31 may be 1000-10000 mm, and the specific length may be selected according to the reaction type, material flow rate, heat transfer and mass transfer, etc. The number of microchannels 31 is 1000-10000, and the specific number may be set according to the output of the production line.
[0058] In some embodiments, Figure 1As shown, the polyacrylonitrile spinning stock solution preparation device of the present invention further includes a polymer raw material storage tank 1 and a polymer raw material feeding pump 11. The polymer raw material feeding pump 11 is used to pump the polymer raw material solution in the polymer raw material storage tank 1 to the polymer raw material solution inlet 101, so that the polymer raw material solution in the microchannel 31 can be automatically fed, which is conducive to the continuous automatic operation of the device of the present invention.
[0059] like Figure 1 As shown, the polyacrylonitrile spinning solution preparation device of the present invention may also include an initiator solution storage tank 2 and an initiator solution feeding pump 10. The initiator solution feeding pump 10 is used to pump the initiator solution in the initiator solution storage tank 2 to the initiator solution inlet 21, so that the initiator solution in the microchannel 31 can be automatically fed, which is conducive to the continuous automatic operation of the device of the present invention.
[0060] It should be noted that the polymerization raw material storage tank 1 and the initiator solution storage tank 2 should both ensure that there is sufficient solution stored at all times to supply the raw materials for the continuous polymerization process. The polymerization raw material feed pump 11 and the initiator solution feed pump 10 can both be metering pumps.
[0061] In some embodiments, Figure 1 As shown, the aforementioned polyacrylonitrile spinning solution preparation device may further include a polymerization buffer tank 5 and a first pump body 12. The solution in the first reaction container 4 can flow into the polymerization buffer tank 5. Specifically, the first reaction container 4 can be located above the polymerization buffer tank 5, and the solution in the first reaction container can flow into the polymerization buffer tank 5 under the action of gravity.
[0062] The first pump body 12 is used to pump at least a portion of the solution in the polymerization buffer tank 5 into the first drainage tube 41, so that the solution repeatedly collides with the first disc 42, and the first disc 42 repeatedly uses centrifugal force and shear force to disperse the polymerization solution into micron-level liquid films and droplets, thereby further enhancing the microscopic mixing performance and heat transfer performance inside the solution, and further narrowing the molecular weight distribution range of polyacrylonitrile.
[0063] It should be noted here that the residence time of the polymerization solution in the first reaction container 4 is relatively short, and the first pump body 12 cooperates with the polymerization buffer tank 5 to ensure that the polymerization solution maintains a relatively long residence time in the first reaction container 4 .
[0064] In some embodiments, Figure 1 As shown, the aforementioned polyacrylonitrile spinning solution preparation equipment also includes a stirring mechanism 51, which is used to stir the solution in the polymerization buffer tank 5, so that the material supplied to the next process is more uniform, thereby improving the processing effect of the next process.
[0065] The above-mentioned cooperation between the microchannel reactor 3 and the circulating reaction device can obtain a preliminary polyacrylonitrile spinning solution with a narrow molecular weight distribution, but there is still a small amount of residual monomers therein. In order to ensure the spinnability of the polyacrylonitrile spinning solution, it is necessary to carry out a stripping and degassing process to remove the residual monomers and bubbles in the spinning solution. The stripping process can be carried out in the stripping device described below, and the degassing process can be carried out in the degassing device described below.
[0066] Specifically, in some embodiments, Figure 1 As shown, the aforementioned polyacrylonitrile spinning solution preparation equipment also includes a single stripping device, which includes a second reaction container 6, a second disc 63, a second drainage tube 61, a second drive mechanism 62 and a first negative pressure mechanism 8. The first negative pressure mechanism 8 is used to evacuate the interior of the second reaction container 6. The first negative pressure mechanism 8 may include a first vacuum pump to evacuate the interior of the second reaction container 6 through the first vacuum pump. Among them, the second disc 63 is arranged in the second reaction container 6, and the second drive mechanism 62 is used to drive the second disc 63 to rotate. Preferably, the center line of the second disc 63 is vertically arranged, and the second disc 63 rotates around its center line. The second drive mechanism 62 includes a second motor to drive the second disc 63 to rotate by the second motor.
[0067] The solution in the polymerization buffer tank 5 can flow into the second drainage pipe 61. Specifically, the inlet of the second drainage pipe 61 is connected to the outlet of the first pump body 12, so that the solution in the polymerization buffer tank 5 is pumped into the second drainage pipe 61 through the first pump body 12. The outlet of the second drainage pipe 61 is opposite to the disk surface of the second disk 63, so that the solution at the outlet of the second drainage pipe 61 can collide with the disk surface of the second disk 63.
[0068] In the above example, the first negative pressure mechanism 8 evacuates the interior of the second reaction container 6 to form a negative pressure, such as a negative pressure of 1-10 kPaa, inside the second reaction container 6. The polymer solution is split into micron-level liquid film droplets by the second disc 63, which greatly increases the specific surface area of the spinning solution and strengthens the continuous removal of some solvents and residual monomers.
[0069] In some embodiments, Figure 1As shown, the aforementioned polyacrylonitrile spinning solution preparation equipment may also include a degassing device. The degassing device includes a third reaction container 7, a third disc 73, a third drainage tube 71, a third driving mechanism 72 and a second negative pressure mechanism 9. The second negative pressure mechanism 9 is used to evacuate the inside of the third reaction container 7. The second negative pressure mechanism 9 may include a second vacuum pump to evacuate the inside of the third reaction container 7 through the second vacuum pump. Among them, the third disc 73 is arranged in the third reaction container 7, and the third driving mechanism 72 is used to drive the third disc 73 to rotate. Preferably, the center line of the third disc 73 is arranged vertically, and the third disc 73 rotates around its center line. The third driving mechanism 72 includes a third motor to drive the third disc 73 to rotate by the third motor.
[0070] The solution in the second reaction container 6 can flow into the third drainage pipe 71. Specifically, Figure 1 As shown, the polyacrylonitrile spinning solution preparation device of the present invention may further include a second pump body 13, and the solution in the second reaction container 6 is pumped into the third drainage pipe 71 through the second pump body 13. The outlet of the third drainage pipe 71 is opposite to the disk surface of the third disk 73, so that the solution at the outlet of the third drainage pipe 71 can collide with the disk surface of the third disk 73.
[0071] In the above example, the second negative pressure mechanism 9 evacuates the interior of the third reaction container 7 to form a negative pressure, such as a negative pressure of 0.5-2 kPaa, inside the third reaction container 7. The third disc 73 provides a larger liquid degassing area for the spinning solution, increases the dynamic degassing area of the material, and is conducive to improving the degassing effect.
[0072] In some embodiments, Figure 1 As shown, the lower part of the third reaction vessel 7 gradually tapers from top to bottom, so that the lower part of the third reaction vessel 7 forms a tower bottom, which can increase the degassing area of the material behind the third disc 73, and can also serve as a buffer device for continuously generating products, which is convenient for feeding the spinning process.
[0073] The polyacrylonitrile spinning stock solution preparation device of the present invention may further include a post-degassing polymer solution delivery pump 14 , and the post-degassing polymer solution delivery pump 14 is used to guide the polyacrylonitrile spinning stock solution in the third reaction container 7 .
[0074] Among them, the polyacrylonitrile spinning solution preparation equipment of the present invention can realize low-viscosity reaction in the microchannel reactor 3 and high-viscosity reaction in the circulating reaction device, so as to enhance the heat transfer and micro-mixing performance of the polymerization process, reduce the equipment construction cost and equipment volume, and greatly improve the process efficiency of the polymerization reaction. In addition, compared with the traditional packed tower, the polymer solution in the second reaction vessel 6 and the third reaction vessel 7 can have a larger gas-liquid contact area by using a disc for de-singling and degassing, which greatly improves the de-singling and degassing efficiency; and it can also reduce the size of the equipment, and can greatly increase the feeding speed.
[0075] The present invention also provides a method for preparing polyacrylonitrile spinning solution, which is used to prepare the polyacrylonitrile spinning solution using any of the above-mentioned polyacrylonitrile spinning solution preparation devices. The preparation method comprises the following steps:
[0076] Prepare a polymerization raw material solution and an initiator solution. The polymerization raw material solution can be prepared by mixing acrylonitrile, a second monomer and dimethyl sulfoxide. The initiator solution can be prepared by mixing an initiator and dimethyl sulfoxide.
[0077] The polymerization raw material solution is introduced into the polymerization raw material solution inlet 101, and the initiator solution is introduced into the initiator solution inlet 21. The temperature of the polymerization raw material solution is higher than the temperature of the initiator solution. Specifically, the temperature of the polymerization raw material solution can be 65-70°C, preferably, the temperature of the polymerization raw material solution is 70°C. The temperature of the initiator solution can be 22-28°C, preferably, the temperature of the initiator solution is 25°C.
[0078] The first driving mechanism 43 drives the first disk 42 to rotate, and the solution at the outlet 301 flows into the first drainage tube 41. The solution at the outlet of the first drainage tube 41 collides with the disk surface of the first disk 42.
[0079] In the above example, after the initiator solution and the polymerization raw material solution both enter the microchannel 31, the temperature of the initiator solution rises rapidly due to the influence of the high-temperature polymerization raw material solution, and the initiator releases free radicals as the temperature rises, so that the free radicals are evenly dispersed in the polymerization raw material solution. Compared with the traditional stirred tank reactor, the heat transfer area provided by the microchannel 31 device increases by 2-3 orders of magnitude, so that the heat generated by the polymerization is promptly transferred to the low-temperature heat transfer medium.
[0080] In some embodiments, the rotation speed of the first disc 42 can be 400-2800 r / min. Preferably, the rotation speed of the first disc 42 is 1000-1500 r / min, so that the first disc 42 can provide sufficient centrifugal force and shear force to stretch and disperse the solution into liquid film and droplets, thereby enhancing internal micro-mixing and reaction heat transfer and mass transfer.
[0081] The feed mass ratio of the polymer raw material solution and the initiator solution at the microchannel 31 can be (4-6): 1. Preferably, the feed mass ratio of the polymer raw material solution and the initiator solution at the microchannel 31 is 6: 1, so that the acrylonitrile in both the polymer raw material solution and the initiator solution can undergo sufficient free radical polymerization reaction under the action of the initiator to obtain the polyacrylonitrile spinning stock solution.
[0082] The average residence time of the above-mentioned polymerization raw material solution and initiator solution in the microchannel 31 is 1-60 minutes. Preferably, the average residence time of the above-mentioned polymerization raw material solution and initiator solution in the microchannel 31 is 20 minutes, so that the polymerization raw material solution and the initiator solution can fully react in the microchannel 31.
[0083] The aforementioned preparation method also includes: introducing the solution in the circulation reactor into the polymerization buffer tank 5, and the first pump body 12 pumps the solution in the polymerization buffer tank 5 into the first drainage tube 41 and the second drainage tube 61 respectively. The mass ratio of the solution pumped into the first drainage tube 41 and the second drainage tube 61 by the first pump body 12 is (20-50):1; preferably, the mass ratio of the solution pumped into the first drainage tube 41 and the second drainage tube 61 by the first pump body 12 is 30:1. By pumping most of the solution in the polymerization buffer tank 5 into the first drainage tube 41, the solution repeatedly collides with the first disc 42, so that the first disc 42 repeatedly uses centrifugal force and shear force to disperse the polymerization solution into liquid films and droplets at the micron level, thereby further enhancing the microscopic mixing performance and heat transfer performance inside the solution, and further narrowing the molecular weight distribution range of polyacrylonitrile.
[0084] The average residence time of the solution at the outlet 301 in the circulation reaction device is 10-120 minutes. Preferably, the average residence time of the solution at the outlet 301 in the circulation reaction device is 60-120 minutes, so that the solution can fully react in the circulation reaction device.
[0085] Further, the solution at the outlet of the second drainage tube 61 collides with the disk surface of the second disk 63. The negative pressure in the second reaction vessel 6 may be 1-10 kPaa. The rotation speed of the second disk 63 may be 400-2800 r / min. Preferably, the rotation speed of the second disk 63 may be 1000-1500 r / min. In this way, the polymer solution can be split into liquid film droplets of micrometer level by the second disk 63, which greatly increases the specific surface area of the spinning solution and strengthens the continuous removal of some solvents and residual monomers.
[0086] The aforementioned preparation method further includes: introducing the solution in the second reaction container 6 into the third drainage tube 71, and the solution at the outlet of the third drainage tube 71 collides with the disk surface of the third disk 73. The negative pressure in the third reaction container 7 is 0.5-2kPaa. The rotation speed of the third disk 73 is 400-2800r / min. Preferably, the rotation speed of the third disk 73 is 400r / min, so that the high rotation speed of the third disk 73 can prevent the spinning solution from entraining bubbles.
[0087] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.
[0088] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.
Claims
1. A polyacrylonitrile spinning solution preparation device, Features: The invention comprises a microchannel reactor (3) and a circulating reaction device, wherein the microchannel reactor (3) comprises a microchannel (31), an inlet arranged at one end of the microchannel (31), and an outlet (301) arranged at the other end of the microchannel; the inlet comprises an initiator solution inlet (21) and a polymerization raw material solution inlet (101); The circulation reaction device comprises a first reaction container (4), a first disc (42), a first drainage tube (41) and a first driving mechanism (43); the first disc (42) is arranged in the first reaction container (4); the first driving mechanism (43) is used to drive the first disc (42) to rotate; the solution at the outlet (301) can flow into the first drainage tube (41); the outlet of the first drainage tube (41) is opposite to the disk surface of the first disc (42), so that the solution at the outlet of the first drainage tube (41) can collide with the disk surface of the first disc (42).
2. The polyacrylonitrile spinning solution preparation device according to claim 1, Features: It also includes a polymerization buffer tank (5) and a first pump body (12), and the solution in the first reaction container (4) can flow into the polymerization buffer tank (5); The first pump body (12) is used to pump at least a portion of the solution in the polymerization buffer tank (5) into the first drainage pipe (41).
3. The polyacrylonitrile spinning solution preparation device according to claim 2, Features: It also comprises a stirring mechanism (51), and the stirring mechanism (51) is used to stir the solution in the polymerization buffer tank (5).
4. The polyacrylonitrile spinning solution preparation device according to claim 2 or 3, Features: It also includes a single-removal device, which includes a second reaction container (6), a second disc (63), a second drainage tube (61), a second driving mechanism (62) and a first negative pressure mechanism (8), wherein the first negative pressure mechanism (8) is used to evacuate the interior of the second reaction container (6); The second disc (63) is arranged in the second reaction container (6), and the second driving mechanism (62) is used to drive the second disc (63) to rotate. The solution in the polymerization buffer tank (5) can flow into the second drainage tube (61), and the outlet of the second drainage tube (61) is opposite to the disk surface of the second disc (63), so that the solution at the outlet of the second drainage tube (61) can collide with the disk surface of the second disc (63).
5. The polyacrylonitrile spinning solution preparation device according to claim 4, Features: The inlet of the second drainage pipe (61) is connected to the outlet of the first pump body (12), so that the solution in the polymerization buffer tank (5) is pumped into the second drainage pipe (61) through the first pump body (12).
6. The polyacrylonitrile spinning solution preparation device according to claim 4, Features: It also includes a degassing device, which includes a third reaction container (7), a third disc (73), a third drainage pipe (71), a third driving mechanism (72) and a second negative pressure mechanism (9), wherein the second negative pressure mechanism (9) is used to evacuate the interior of the third reaction container (7); The third disk (73) is arranged in the third reaction container (7), and the third driving mechanism (72) is used to drive the third disk (73) to rotate. The solution in the second reaction container (6) can flow into the third drainage tube (71), and the outlet of the third drainage tube (71) is opposite to the disk surface of the third disk (73), so that the solution at the outlet of the third drainage tube (71) can collide with the disk surface of the third disk (73).
7. The polyacrylonitrile spinning solution preparation device according to claim 6, Features: It also includes a second pump body (13), through which the solution in the second reaction container (6) is pumped into the third drainage tube (71).
8. The polyacrylonitrile spinning solution preparation device according to claim 6 or 7, Features: The lower part of the third reaction container (7) gradually becomes thinner from top to bottom.
9. The polyacrylonitrile spinning solution preparation device according to any one of claims 1-3 and 5-7, Features: The polyacrylonitrile spinning stock solution preparation device further comprises a polymer raw material storage tank (1) and a polymer raw material feeding pump (11), wherein the polymer raw material feeding pump (11) is used to pump the polymer raw material solution in the polymer raw material storage tank (1) to the polymer raw material solution inlet (101); And / or, the polyacrylonitrile spinning solution preparation equipment also includes an initiator solution storage tank (2) and an initiator solution feeding pump (10), and the initiator solution feeding pump (10) is used to pump the initiator solution in the initiator solution storage tank (2) to the initiator solution inlet (21).
10. A method for preparing polyacrylonitrile spinning solution, using the polyacrylonitrile spinning solution preparation device according to any one of claims 1 to 9, Features: The preparation method comprises the following steps: preparing a polymerization raw material solution and an initiator solution; Introducing a polymerization raw material solution into the polymerization raw material solution inlet (101), and introducing the initiator solution into the initiator solution inlet (21); wherein the temperature of the polymerization raw material solution is higher than the temperature of the initiator solution; The first driving mechanism (43) drives the first disc (42) to rotate, and the solution at the outlet (301) flows into the first drainage tube (41), and the solution at the outlet of the first drainage tube (41) collides with the disc surface of the first disc (42).
11. The method for preparing polyacrylonitrile spinning solution according to claim 10, Features: The rotation speed of the first disc (42) is 400-2800 r / min; And / or, the feed mass ratio of the polymerization raw material solution to the initiator solution at the microchannel (31) is (4-6):1; And / or, the average residence time of the polymerization raw material solution and the initiator solution in the microchannel (31) is 1-60 minutes.
12. The method for preparing polyacrylonitrile spinning solution according to claim 10 or 11, Features: The preparation method further comprises: introducing the solution in the circulation reactor into the polymerization buffer tank (5), and the first pump body (12) pumping the solution in the polymerization buffer tank (5) into the first drainage pipe (41) and the second drainage pipe (61) respectively; Wherein, the mass ratio of the solution pumped into the first drainage tube (41) and the second drainage tube (61) by the first pump body (12) is (20-50):1; and / or, the average residence time of the solution at the outlet (301) in the circulation reaction device is 10-120 minutes.
13. The method for preparing polyacrylonitrile spinning solution according to claim 12, Features: The solution at the outlet of the second drainage tube (61) collides with the disk surface of the second disk (63); Wherein, the negative pressure in the second reaction container (6) is 1-10 kPaa; and / or the rotation speed of the second disc (63) is 400-2800 r / min.
14. The method for preparing polyacrylonitrile spinning solution according to claim 12, Features: The preparation method further comprises: introducing the solution in the second reaction container (6) into the third drainage tube (71), and the solution at the outlet of the third drainage tube (71) collides with the disk surface of the third disk (73); Wherein, the negative pressure in the third reaction container (7) is 0.5-2 kPaa; and / or the rotation speed of the third disc (73) is 400-2800 r / min.
15. The method for preparing polyacrylonitrile spinning solution according to any one of claims 10-11, 13-14, Features: The polymerization raw material solution is prepared by mixing acrylonitrile, a second monomer and dimethyl sulfoxide; and / or, the temperature of the polymerization raw material solution is 65-70° C.; And / or, the initiator solution is prepared by mixing an initiator and dimethyl sulfoxide; And / or, the temperature of the initiator solution is 22-28°C.
Citation Information
Cited By
Polyacrylonitrile spinning solution and preparation method and device therefor, and polyacrylonitrile carbon fiber precursor
WO2026108582A1