Iron-nickel co-doped porous carbon nanoparticle and nanotube hybrid material as well as preparation method and application thereof
By using iron-nickel co-doped porous carbon nanoparticles and nanotube hybrid materials, the problems of secondary pollution and high energy consumption caused by metal leaching in traditional advanced oxidation methods have been solved, achieving efficient and low-cost degradation of organic pollutants.
Patent Information
- Application Number
- CN202411003690.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-25
Smart Images

Figure CN118874471A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material preparation, and specifically relates to an iron-nickel co-doped porous carbon nanoparticle and nanotube hybrid material, a preparation method thereof, and its application in the field of polluted water restoration for catalytic degradation of organic pollutants. Background Art
[0002] Pollutants such as antibiotics and organic dyes exist in large quantities in the water environment because they cannot be biodegraded. Based on their ability to accumulate in water bodies for a long time, they pose huge risks to the ecosystem and human health. At present, advanced oxidation processes have a significant effect on degrading organic pollutants in water.
[0003] Advanced Oxidation Processes (AOPs) have shown excellent performance in the removal of organic pollutants. Advanced oxidation processes have the ability to produce strong oxidizing substances, which can decompose organic pollutants into low-toxic or non-toxic small molecules, and can even mineralize them into carbon dioxide and water. However, traditional advanced oxidation methods, such as the Fenton oxidation method, will produce a large amount of iron sludge, the utilization rate of hydrogen peroxide activation method is low, and ultraviolet activation and thermal activation have high energy consumption and high cost, which limits their practical application. Activated persulfate is a new type of advanced oxidation technology, in which transition metal materials (such as iron, cobalt, copper, nickel, etc.) have been proven to be able to efficiently activate PMS, but during the use of metal-doped catalysts, secondary pollution is easily caused by the leaching of metal ions. Therefore, it is necessary to find a suitable carrier to wrap the transition metal inside it to form a composite material with nano-constraints to solve this problem.
[0004] In addition, through the search of existing technical literature, it was found that Liu Ying et al. published a metal organic framework-derived nitrogen-doped porous Co@C nanobox in the Journal of Environmental Engineering 2019, 02 to activate persulfate to efficiently remove p-chloroaniline; He Yangzhuo et al. published a ZIF-derived copper-cobalt-zinc oxide in the carbon framework to limit the degradation of organic pollutants in the Journal of Hazardous Substances 2022, 440; Ye Jian et al. published a core-shell ZIF-67 / ZIF-8-derived sea urchin-like cobalt / nitrogen co-doped carbon nanotube hollow framework with ultra-high adsorption and catalytic activity in the Journal of the Chinese Society of Chemical Engineering 2020, 112; there are also reports on some carbon nanotube and nanoparticle hybrid materials as activators. Both carbon nanotubes and nanoparticles have the characteristics of high specific surface area and high graphitization, can provide a large number of active sites, have strong electronic conductivity, acid and alkali resistance, etc., and are currently a hot topic of research. Although there are many methods for synthesizing this type of hybrid materials, the processes are relatively complicated. Summary of the invention
[0005] In view of this, the present invention has developed an iron-nickel co-doped porous carbon nanoparticle and nanotube hybrid material, using MOF as a precursor and co-doping with iron and nickel. The carbon nanoparticle and carbon nanotube hybrid material formed can solve the metal leaching problem while also having good degradation performance, and can be used as a more ideal material for activating PMS to degrade organic pollutants.
[0006] It should be noted that the present invention, through the synergistic effect of a small amount of transition metals on ZIF-8, generates metal particles encapsulated inside carbon nanoparticles and carbon nanotube hybrid materials, aiming to provide a new method for synthesizing carbon nanoparticles and carbon nanotube hybrid materials to solve the problems of long time, high energy consumption, and complicated reactions in traditional methods.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The first technical purpose of the present invention is to provide a method for preparing an Fe-Ni co-doped porous carbon nanoparticle and nanotube hybrid material, the method specifically comprising the following steps:
[0009] (1) ZIF-8 prepared by conventional method [1] , iron salt and nickel salt are poured into a beaker containing deionized water, stirred for reaction, filtered and freeze-dried for later use;
[0010] (2) placing the freeze-dried powder of step (1) in a tube furnace, calcining it under the protection of nitrogen or argon, and naturally cooling it to room temperature to finally obtain the iron-nickel co-doped porous carbon nanoparticles and nanotube hybrid material.
[0011] Optionally, the quantitative ratio of ZIF-8, iron salt and nickel salt is 6-10:0.5-1:0.5-2.
[0012] Furthermore, the iron salt is ammonium ferrous sulfate, and the nickel salt is nickel sulfate or nickel nitrate.
[0013] Optionally, in step (1), the reaction temperature is room temperature, and the reaction time is 0.5 to 2 h; the freeze-drying temperature is -15 to -30°C, and the time is 6 to 12 h.
[0014] Optionally, the roasting process parameters in step (2) are: heating to 750-950° C. at a heating rate of 1-5° C. / min and maintaining for 2-4 hours.
[0015] The second technical purpose of the present invention is to provide an iron-nickel co-doped porous carbon nanoparticle and nanotube hybrid material prepared by the method described above, which is a hierarchical porous carbon material formed by mutual hybridization of carbon nanoparticles and carbon nanotubes.
[0016] The third technical purpose of the present invention is to provide the use of the iron-nickel co-doped porous carbon nanoparticles and nanotube hybrid materials prepared by the method as described above in the restoration of polluted water bodies.
[0017] Specifically, the iron-nickel co-doped porous carbon nanoparticles and nanotube hybrid material can be used as an activated PMS to degrade organic pollutants in water.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. In the present invention, the doped metal particles are wrapped inside the carbon nanotubes and carbon nanosheets, thus avoiding the secondary pollution problem caused by metal leaching.
[0020] 2. In the present invention, by providing a small amount of metal, under the synergistic effect of ZIF-8, a hybrid material of carbon nanoparticles and carbon nanotubes encapsulating metal is formed, which solves the problems of high energy consumption, high cost, and complicated reaction in the traditional method.
[0021] 3. In the present invention, the carbon nanotubes and the carbon nanoparticles and carbon nanotubes are entangled and interconnected to form a three-dimensional conductive network, which is conducive to the transfer of electrons between PMS and organic pollution, thereby degrading organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0023] Figure 1 The present invention provides a process flow chart for preparing the iron-nickel co-doped porous carbon nanoparticles and nanotube hybrid materials.
[0024] Figure 2 This is the SEM image of FeNi-NC / CNT obtained in Example 1.
[0025] Figure 3 This is the TEM image of FeNi-NC / CNT obtained in Example 1.
[0026] Figure 4 This is the adsorption-desorption curve of FeNi-NC / CNT obtained in Example 1.
[0027] Figure 5 This is the pore size distribution diagram of FeNi-NC / CNT obtained in Example 1.
[0028] Figure 6This is the XPS graph of FeNi-NC / CNT obtained in Example 1.
[0029] Figure 7 This is a performance diagram of the degradation of organic pollutants in water by FeNi-NC / CNT, FeNi-NC / CNT-0.5, and FeNi-NC / CNT-2 obtained in Examples 1-3.
[0030] Figure 8 This is a comparison chart of the degradation performance of organic pollution in water by FeNi-NC / CNT, Fe-NC / CNT, Ni-NC / CNT, and NC / CNT obtained in Example 1 and Comparative Examples 1-3.
[0031] Fig. 9 This is a performance diagram of the FeNi-NC / CNT obtained in Example 1 in degrading different pollutants in water.
[0032] Fig.10 This is a diagram showing the cyclic effect of FeNi-NC / CNT prepared in Example 1 activating PMS to degrade SDZ. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0035] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0036] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0037] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0038] The invention discloses the preparation of an iron-nickel co-doped porous carbon nanoparticle and nanotube hybrid material and the application of the hybrid material in activating persulfate to efficiently degrade organic pollutants in water.
[0039] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0040] Example 1: Preparation of FeNi-NC / CNT
[0041] Step 1. Prepare ZIF-8 by conventional method [1] , iron salt and nickel salt are weighed in a mass ratio of 9:1:1 = 0.5220g:0.058g:0.058g, poured into a beaker containing a small amount of deionized water, stirred for 1 hour, and filtered.
[0042] Step 2. Place the powder obtained by filtration in step 1 in a freeze dryer and freeze-dry under vacuum at -30°C for 6 hours.
[0043] Step 3. Place the freeze-dried powder in step 2 in a tube furnace, and under the protection of nitrogen or argon, heat the temperature to 950°C at a rate of 5°C / min and maintain for 3 hours. After completion, naturally cool to room temperature, take out, wash and dry to obtain FeNi-NC / CNT.
[0044] The pore volume of FeNi-NC / CNT obtained is 1.16 cm 3 / g, pore diameter 44.2nm, specific surface area 513.9cm 2 / g. And, by Figure 2 The SEM image shows that the carbon nanoparticles and carbon nanotubes of the material are hybridized. Figure 3 From the TEM image, it can be observed that the metal nanoparticles are encapsulated inside the carbon material and the material has graphitized carbon.
[0045] Depend on Figure 6 It can be seen that there are five N configurations in FeNi-NC / CNT: pyridinic N (398.4 eV), Fe / Ni-N4 (398.9 eV), pyrrolic N (399.7 eV), graphitic N (401 eV), and oxidized N (403.2 eV). 2+ 2p, Fe 3+ 2p, Fe 0 Nickel exists in the form of Ni2+ 2p,Ni 3+ 2p,Ni 0 This indicates the successful doping of Fe and Ni atoms.
[0046] Document 1: Wang Q, Guan Z, Xiong Y, Li D. Nanoconfinement-enhanced Fenton-like polymerization via hollow hetero-shell carbon for reducing carbonemissions in organic wastewater purification. Journal of ColloidandInterfaceScience 2023;634:231-242.
[0047] Example 2: Preparation of FeNi-NC / CNT-0.5
[0048] Compared with Example 1, the present embodiment is different in that in step 1, materials are weighed according to the mass ratio of ZIF-8: iron salt: nickel salt = 9: 0.5: 1 = 0.5220 g: 0.029 g; 0.058 g.
[0049] Example 3: Preparation of FeNi-NC / CNT-2
[0050] The difference between this embodiment and embodiment 1 is that in step 1, the materials are weighed according to the mass ratio of ZIF-8: iron salt: nickel salt = 9: 1: 0.5 = 0.522 g: 0.058 g: 0.029 g.
[0051] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples and experimental examples are used to further illustrate the technical features disclosed in the present invention, but they should not be understood as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without creative work are also considered to fall within the scope of protection of the present invention.
[0052] Comparative Example 1: Preparation of Fe-NC / CNT
[0053] The difference between this comparative example and Example 1 is that no nickel salt is added in step 1, and the other proportions remain unchanged.
[0054] Comparative Example 2: Preparation of Ni-NC / CNT
[0055] Compared with Example 1, in this comparative example, no iron salt is added in step 1, and the other proportions remain unchanged.
[0056] Comparative Example 3: Preparation of NC / CNT
[0057] The difference between this comparative example and Example 1 is that neither iron salt nor nickel salt is added, and ZIF-8 is directly fired.
[0058] Experimental Example 1:
[0059] This experimental example provides a performance test of the first catalytic degradation of organic pollutants in water by FeNi-NC / CNT, FeNi-NC / CNT-0.5, and FeNi-NC / CNT-2 prepared in Examples 1-3, including the following steps:
[0060] (1) Prepare 50 mL of a 10 mg / L solution of sulfadiazine (SDZ) and transfer it into a 100 mL beaker without adjusting the pH.
[0061] (2) Accurately weigh 5 mg of the materials prepared in Examples 1-3 and add them to a beaker. Place the beaker on a magnetic stirring table and stir at 180 rpm and 25° C. Add 1 mL of 0.05 mol / L potassium persulfate to the mixture of the catalyst and SDZ to start the catalytic degradation reaction. Samples are taken at certain time intervals to test the concentration. Figure 7 It can be seen that Examples 1-3 all have good degradation effects on SDZ, and the degradation rates of SDZ can reach 90% within 20 minutes.
[0062] Experimental Example 2:
[0063] This experimental example provides the first catalytic degradation performance test of organic pollutants in water by FeNi-NC / CNT, Fe-NC / CNT, Ni-NC / CNT, and NC / CNT prepared in Example 1 and Comparative Examples 1-3.
[0064] The specific operation steps are the same as those in Experimental Example 1. Figure 8 As shown, in this experimental example, the FeNi-NC / CNT obtained in Example 1 has the best degradation effect on SDZ and can completely degrade SDZ within 20 minutes, while the degradation efficiency of the materials obtained in the comparative examples on SDZ is less than 70%.
[0065] Experimental Example 3:
[0066] This experimental example provides a performance test of FeNi-NC / CNT prepared in Example 1 for degrading different organic pollutants, including the following steps:
[0067] (1) Prepare 50 mL and 10 mg / L solutions of rhodamine B (RhB), methylene blue (MB), tetracycline (TC), and sulfamethoxazole (SMX), respectively, and transfer them into a 100 mL beaker.
[0068] (2) Accurately weigh 5 mg of FeNi-NC / CNT and put it into a beaker. Then put a stirrer into the beaker and stir it on a magnetic stirring table at 180 rpm and 25 °C. Add 1 mL of 0.05 mol / L potassium persulfate to the mixture of catalyst and SDZ. Samples are taken at certain time intervals to test the concentration. Fig. 9 It can be seen that for different pollutants, the FeNi-NC / CNT prepared in Example 1 can be almost completely degraded within 20 minutes.
[0069] Experimental Example 4:
[0070] This experimental example provides a cycle experiment of preparing FeNi-NC / CNT in Example 1 to prove that the prepared material has good stability; the specific steps are as follows:
[0071] (1) The solution after the reaction in Experimental Example 3 was filtered, and the obtained powder material was the FeNi-NC / CNT prepared in Example 1 after use, which was placed in a vacuum oven at 80° C. for drying.
[0072] (2) Take 5 mg of the dried Example 1 material in a 100 mL beaker, take 50 mL of a 10 mg / L SDZ solution, do not adjust the pH, and transfer it to a 100 mL beaker. Place a stir bar in the beaker and stir it on a magnetic stirring table at 180 rpm and 25°C. Add 1 mL of 0.05 mol / L potassium persulfate to the mixture of the catalyst and SDZ to start the catalytic degradation reaction. Take samples at certain time intervals to test the concentration. Repeat the above operation to perform a cyclic experiment. Fig.10 As shown, after 5 cycles, the degradation efficiency of FeNi-NC / CNT obtained in Example 1 for SDZ can still reach 90%, indicating that BC-NS has good stability and reusability and good economic benefits.
[0073] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a hybrid material of iron-nickel co-doped porous carbon nanoparticles and nanotubes, It is characterized in that The method specifically comprises the following steps: (1) Pour ZIF-8, iron salt and nickel salt prepared by conventional method into deionized water, stir to react, filter and freeze-dry for later use; (2) calcining the freeze-dried powder in step (1) under the protection of nitrogen or argon, and naturally cooling to room temperature to finally obtain the iron-nickel co-doped porous carbon nanoparticles and nanotube hybrid material.
2. The method for preparing the Fe-Ni co-doped porous carbon nanoparticles and nanotube hybrid material according to claim 1, It is characterized in that The quantitative ratio of the ZIF-8, iron salt and nickel salt is 6-10:0.5-1:0.5-2.
3. The method for preparing the hybrid material of iron-nickel co-doped porous carbon nanoparticles and nanotubes according to claim 1 or 2, It is characterized in that The iron salt is ammonium ferrous sulfate, and the nickel salt is nickel sulfate or nickel nitrate.
4. The method for preparing the Fe-Ni co-doped porous carbon nanoparticles and nanotube hybrid material according to claim 1, It is characterized in that In the step (1), the reaction temperature is room temperature and the reaction time is 0.5 to 2 hours; the freeze-drying temperature is -15 to -30°C and the time is 6 to 12 hours.
5. The method for preparing the Fe-Ni co-doped porous carbon nanoparticles and nanotube hybrid material according to claim 1, It is characterized in that The roasting process parameters in step (2) are as follows: Increase the temperature to 750-950°C at a heating rate of 1-5°C / min and maintain for 2-4h.
6. An Fe-Ni co-doped porous carbon nanoparticle and nanotube hybrid material prepared by the method of claim 1, It is characterized in that Carbon nanoparticles and carbon nanotubes are hybridized to form hierarchical porous carbon materials.
7. Use of the iron-nickel co-doped porous carbon nanoparticles and nanotube hybrid material prepared by the method of claim 1 or the iron-nickel co-doped porous carbon nanoparticles and nanotube hybrid material as claimed in claim 6 in the remediation of polluted water bodies.
8. The use according to claim 7, wherein the iron-nickel co-doped porous carbon nanoparticles and nanotube hybrid materials can be used as activated PMS to degrade organic pollutants in water.
Citation Information
Patent Citations
Bamboo-like carbon nanotube / hierarchical porous biochar composite material and preparation method thereof
CN111068736A
Carbon nanotube and graphite flake hybrid material and preparation method and application thereof
CN112264000A
Novel compounding method of carbon material and transition metal compound, composite material and application
CN113629245A
g-C3N4-doped nanotube photocatalyst as well as preparation method and application thereof
CN114054066A
Lignite-based nitrogen-doped iron carbide and graphite carbon layer / carbon nanotube hybrid material as well as preparation method and application thereof
CN116130682A