Bimetal doped biochar catalyst and preparation method thereof
By preparing poultry and livestock manure into poultry and livestock manure into porous structures, loading ZnO, Fe0 and Fe3O4, the problem of difficult-to-degrade organic pollutants in water treatment is solved, and efficient and low-cost pollutant removal is achieved Effect.
Patent Information
- Application Number
- CN202410849083.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to effectively remove difficult-to-degrade organic pollutants in water treatment, especially methane and other organic matter produced after poultry and livestock manure treatment, and the activation persulfate technology has challenges such as activator selection and side reaction control.
Develop a bimetal doped biochar catalyst (ZnFeBC) to improve the catalyst by preparing poultry and livestock manure into biochar with porous structure and loading ZnO, Fe0 and Fe3O4 on its surface. specific surface area and ability to activate persulfate.
The activated persulfate properties of the catalyst are significantly improved, efficient removal of pollutants in water is achieved, and the cost is reduced. The removal rate of the catalyst for thiamethoxam reaches 100%, which has excellent activation properties and environmentally friendly characteristics.
Smart Images

Figure CN118874474A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment, and specifically relates to a bimetallic doped biochar catalyst and a preparation method thereof. Background Art
[0002] With the rapid development of agriculture and animal husbandry, the increase in the number of livestock and poultry has provided us with abundant food resources, but it will also produce a large amount of feces. Livestock and poultry feces are rich in organic matter, nitrogen, phosphorus and other nutrients. If not handled properly, it will not only waste resources, but also cause serious pollution to the environment. Untreated livestock and poultry feces discharged directly into the environment will cause groundwater and water pollution. In addition, when livestock and poultry feces decompose, they will produce greenhouse gases such as methane, which will have an adverse effect on global climate change. At the same time, if livestock and poultry feces are piled up over a large area, it may become a breeding ground for pests and diseases, posing a threat to public health and safety.
[0003] Although livestock manure treatment is an environmental issue, it can also bring new opportunities for my country's agricultural and energy development. Using livestock manure, a widely available resource, to prepare biochar can not only alleviate environmental pollution problems, but also provide efficient and green catalytic solutions for related industries. In addition, this also provides breeders and farmers with an economical and effective method for livestock manure treatment, achieving dual economic and environmental benefits.
[0004] With the acceleration of industrialization and the growth of population, various organic pollutants in water bodies have gradually become prominent. These organic pollutants are difficult to be completely degraded or removed in traditional water treatment methods, and these refractory organic matter may pose a serious threat to human health and the ecological environment. In order to more effectively remove these refractory organic matter, researchers have developed a series of advanced oxidation technologies (AOPs). The main working mechanism is to generate highly active hydroxyl radicals. Hydroxyl radicals are very powerful oxidants that can quickly and non-selectively mineralize or degrade most organic pollutants in a short period of time. One of the methods is activated persulfate. Its principle is to use an activator, such as transition metals, ultraviolet rays or strong oxidants, to activate persulfate (also known as peroxysulfate) to produce hydroxyl radicals, thereby achieving the degradation of organic pollutants. Due to the simplicity, low cost and easy operation of this method, activated persulfate technology has been widely used in the treatment of industrial and domestic sewage. Although activated persulfate technology has obvious advantages, it also faces some challenges, such as the selection of activators, the control of side reactions and the optimization of operating conditions.
[0005] Biochar has great potential in environmental governance due to its wide sources, simple preparation methods, low cost, high stability, large specific surface area, and large adsorption capacity. Studies have shown that the functional groups on the surface of biochar also have a certain degree of activation effect on persulfate. Preparing livestock manure into biochar can not only realize the resource utilization of livestock manure waste, but also use it in wastewater treatment. Bimetallic modification of biochar materials can significantly improve its activation effect on persulfate.
[0006] In summary, there is an urgent need to develop a biochar catalyst to address the defects in existing technologies. Summary of the invention
[0007] To solve the above problems, the present invention provides a bimetallic doped biochar catalyst and a preparation method thereof, which can effectively improve the performance of the biochar catalyst in activating persulfate, save application costs, be environmentally friendly and efficient, and achieve the removal of pollutants in water.
[0008] One object of the present invention is to provide a bimetallic doped biochar catalyst (ZnFeBC catalyst), wherein the bimetallic doped biochar catalyst comprises biochar having a porous structure, and ZnO, Fe 0 (zero-valent iron), Fe2O3 and Fe3O4.
[0009] Furthermore, the specific surface area of the bimetallic doped biochar catalyst is 130-150m 2 / g.
[0010] Furthermore, the pore size of the biochar is 10-14 nm.
[0011] Furthermore, the raw material of the biochar is livestock manure.
[0012] Preferably, the raw material of the biochar is cow dung.
[0013] The present invention also provides a method for preparing the bimetallic doped biochar catalyst, comprising the following steps:
[0014] S1, adding livestock manure, zinc salt and K2FeO4 into water, heating, stirring and grinding to obtain a mixed powder;
[0015] S2. Under the protection of an inert gas, the mixed powder is carbonized and purified to obtain a bimetallic doped biochar catalyst (ZnFeBC catalyst).
[0016] Preferably, the zinc salt is ZnCl2.
[0017] Furthermore, in step S1, the heating temperature is 75-85°C.
[0018] Furthermore, in step S2, the temperature of the carbonization treatment is 500-700°C, and the time is 1.5-4h.
[0019] Furthermore, in step S2, the temperature rising rate is 3-7°C / min.
[0020] Specifically, in step S1, the mixed powder also needs to be filtered through a 60-70 mesh sieve.
[0021] Specifically, in step S2, during the carbonization process, sulfuric acid solution is also required to absorb tail gas;
[0022] Wherein, the volume ratio of sulfuric acid to water in the sulfuric acid solution is 1-2:3-5.
[0023] The present invention also provides application of the bimetallic doped biochar catalyst in water treatment.
[0024] Specifically, the ZnFeBC catalyst of the present invention has an excellent removal effect on thiamethoxam (THM), with the highest removal rate reaching 100%;
[0025] The specific treatment method is as follows: ZnFeBC catalyst and persulfate are added to the thiamethoxam solution at the same time, and the reaction is stirred for 60-70 minutes to remove organic pollutants.
[0026] Preferably, when the thiamethoxam content is 20 mg / L, the dosage of the ZnFeBC catalyst is 0-1.0 g / L, and the dosage of the persulfate is 0-1.5 g / L.
[0027] Preferably, the degradation environment temperature is 20-30°C and the pH is 3-11.
[0028] The present invention has the following beneficial effects:
[0029] 1. The biochar raw material in the present invention has the characteristics of wide source, low price and abundant output. Meanwhile, the ZnFeBC catalyst has the characteristics of low preparation cost, environmental friendliness and excellent activation performance, and can be used for efficient degradation of pollutants in the environment.
[0030] 2. Compared with pure biochar BC catalyst or zinc-modified biochar ZnBC catalyst, the biochar is modified by using zinc salt and K2FeO4, so that the surface of the prepared ZnFeBC catalyst has abundant functional groups. The two together improve the original structure of the material, increase the specific surface area of the ZnFeBC catalyst, and increase the pores on the ZnFeBC catalyst, which is conducive to providing more active sites; at the same time, the Fe loaded on the ZnFeBC catalyst 0And Fe3O4 provide dual active sites for catalyzing PMS, accelerate electron transfer, increase reaction rate, improve reaction selectivity, and increase the utilization of active sites, which synergistically enhance the catalytic performance of the catalyst, making it have excellent activation performance, and can activate persulfate to produce free radicals, thereby performing advanced oxidation degradation of pollutants, and has an excellent removal effect on pollutants in the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The effect of different catalyst dosages on THM removal efficiency;
[0032] Figure 2 The effect of different PMS dosage on THM removal rate;
[0033] Figure 3 is the effect of environmental pH on THM removal rate;
[0034] Figure 4 The effect of different calcination temperatures on the catalytic performance of the catalyst;
[0035] Figure 5 The removal rate of THM by catalytic degradation of PMS by catalysts prepared with different raw material mass ratios;
[0036] Figure 6 is the removal rate of THM degradation by different biochar catalysts;
[0037] Figure 7 The XRD patterns of ZnFeBC, BC, and ZnFeBC biochar catalysts are compared;
[0038] Figure 8 Comparison of FTIR images of ZnFeBC, BC, and ZnFeBC biochar catalysts;
[0039] Fig. 9 The adsorption configuration of the ZnFeBC catalyst and PMS in Example 1;
[0040] Fig.10 is a SEM image of the ZnFeBC catalyst of Example 1;
[0041] Fig.11 is the SEM image of the BC catalyst of Comparative Example 1;
[0042] Fig.12 This is the SEM image of the ZnBC catalyst of Comparative Example 2. DETAILED DESCRIPTION
[0043] In order to more clearly illustrate the technical solution of the present invention, the following examples are listed. Unless otherwise stated, the raw materials, reactions and post-treatment methods shown in the examples are common raw materials on the market and technical methods well known to those skilled in the art.
[0044] The words "preferred", "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that can provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.
[0045] It should be understood that, except in any operating examples, or where otherwise indicated, all numbers expressing, for example, the amounts of ingredients used in the specification and claims should be understood to be modified in all instances by the term "about". Therefore, unless indicated to the contrary, the numerical parameters set forth in the following specification and the appended claims are approximate values that vary depending on the desired properties to be obtained by the present invention.
[0046] Cow dung was purchased from a dairy farm in Nan'an City, Fujian Province.
[0047] THM stock solution was purchased from Shanghai Anpu Experimental Technology Co., Ltd. with a concentration of 95 wt%.
[0048] Example 1
[0049] A bimetallic doped biochar catalyst, the bimetallic doped biochar catalyst comprising biochar, the biochar having a porous structure, the biochar loaded with ZnO, Fe 0 , Fe2O3 and Fe3O4.
[0050] The preparation method of the bimetallic doped biochar catalyst comprises the following steps:
[0051] S1-1, air-dry the cow dung, grind it, and pass it through a 60-mesh sieve;
[0052] S1-2, add 12g of cow dung, 6g of ZnCl2 and 12g of K2FeO4 into deionized water, heat to 80°C, stir until dry, grind into powder, and filter through a 60-mesh sieve to obtain a mixed powder;
[0053] S2. Place the mixed powder into a tubular furnace, introduce nitrogen into the tubular furnace, and evacuate the furnace three times with an air pump, continue to introduce nitrogen, and carbonize the mixed powder for 2 hours at a heating rate of 5°C / min and a calcination temperature of 700°C. After cooling, wash the mixed powder alternately with water and ethanol and centrifuge it three times, and then dry it in an oven at 105°C to obtain a bimetallic doped biochar catalyst (ZnFeBC catalyst).
[0054] Fig.10 This is a SEM image of the ZnFeBC catalyst of Example 1 of the present invention. It can be seen that the surface of the ZnFeBC catalyst is loaded with a petal-shaped crystal structure.
[0055] Example 2
[0056] The difference between this embodiment and embodiment 1 is that in step S1, the mass ratio of cow dung, ZnCl2 and K2FeO4 is 2:1:1, and the other components and preparation method are the same as those in embodiment 1.
[0057] Example 3
[0058] The difference between this embodiment and embodiment 1 is that in step S2, the calcination temperature is 500°C, and the other components and preparation method are the same as those in embodiment 1.
[0059] Example 4
[0060] The difference between this embodiment and embodiment 1 is that in step S2, the calcination temperature is 600°C, and the other components and preparation method are the same as those in embodiment 1.
[0061] Comparative Example 1
[0062] Preparation of BC catalyst
[0063] The difference between this comparative example and Example 1 is that ZnCl2 and K2FeO4 are not added in step S1-2, and the other components and preparation method are the same as those in Example 1.
[0064] Fig.11 This is the SEM image of the BC catalyst of Comparative Example 1. It can be seen that the surface of BC is relatively smooth and has fewer pores. Comparative Example 2
[0065] Preparation of ZnBC catalyst
[0066] The difference between this comparative example and Example 1 is that K2FeO4 is not added in step S1-2, and the other components and preparation method are the same as those in Example 1.
[0067] Fig.12 This is the SEM image of the ZnBC catalyst of Comparative Example 2. It can be seen that the surface of ZnBC is rough, with many pores and a complex pore structure.
[0068] Comparative Example 3
[0069] Preparation of FeBC catalyst
[0070] The difference between this comparative example and Example 1 is that ZnCl2 is not added in step S1-2, and the other components and preparation method are the same as those in Example 1.
[0071] Test Example 1
[0072] The effect of the dosage of the ZnFeBC catalyst prepared in Example 1 on the THM (thiamethoxam) removal rate was investigated.
[0073] Test method:
[0074] Step A1: prepare a THM stock solution with a concentration of 200 ppm using deionized water, take 10 ml of the THM stock solution into a 250 ml beaker, add 90 ml of deionized water, and stir and dilute to obtain a THM solution with a concentration of 20 ppm;
[0075] Step A2: at room temperature and pH=7, place a beaker on a magnetic stirrer, add the ZnFeBC catalyst of Example 1 and 1.2 mg of PMS oxidant (potassium persulfate oxidant) to the THM solution, stir evenly, and degrade THM in the THM solution;
[0076] Wherein, the dosage of the ZnFeBC catalyst is 0mg, 0.2mg, 0.5mg, 0.75mg, and 1.0mg respectively;
[0077] Step A3: Starting from the moment when the ZnFeBC catalyst and the PMS oxidant are added, within a given reaction interval (0 min, 5 min, 10 min, 20 min, 30 min, 60 min), 0.3 mL of the THM solution is transferred into a small centrifuge tube, filtered through a 0.22 um filter membrane, and then 100 ul is transferred from the small centrifuge tube into a sample injection vial using a 100 ul pipette, and immediately quenched with 0.1 ml of methanol, and finally 0.8 ml of deionized water is added, vortexed, and a mixed solution is obtained;
[0078] Step A4: Repeat step A2 three times, and use high performance liquid chromatography (HPLC) to determine the concentration of THM in the three mixed solutions, and take the average value.
[0079] The test results are as follows Figure 1As shown, it can be seen that when the ZnFeBC catalyst dosage is in the range of 0-0.75g / L, the THM removal rate increases with the increase of the ZnFeBC catalyst dosage. When the ZnFeBC catalyst dosage is 0.75g / L, the THM removal rate reaches 100% within 60min, and when the ZnFeBC catalyst dosage increases to 1.0g / L, the THM removal rate decreases instead.
[0080] Test Example 2
[0081] The effect of the dosage of PMS oxidant on THM removal rate was investigated.
[0082] Test method:
[0083] Step A1: prepare a THM stock solution with a concentration of 200 ppm using deionized water, take 10 ml of the THM stock solution into a 250 ml beaker, add 90 ml of deionized water, and stir and dilute to obtain a THM solution with a concentration of 20 ppm;
[0084] Step A2: at room temperature and pH=7, place a beaker on a magnetic stirrer, add 0.75 mg of the ZnFeBC catalyst of Example 1 and the PMS oxidant to the THM solution, stir evenly, and degrade the THM in the THM solution;
[0085] Wherein, the dosage of the PMS oxidant is 0 mg, 0.2 mg, 0.5 mg, 1.0 mg, and 1.5 mg respectively;
[0086] Step A3: Starting from the moment when the ZnFeBC catalyst and the PMS oxidant are added, within a given reaction interval (0 min, 5 min, 10 min, 20 min, 30 min, 60 min), 0.3 mL of the THM solution is transferred into a small centrifuge tube, filtered through a 0.22 um filter membrane, and then 100 ul is transferred from the small centrifuge tube into a sample injection vial using a 100 ul pipette, and immediately quenched with 0.1 ml of methanol, and finally 0.8 ml of deionized water is added, vortexed, and a mixed solution is obtained;
[0087] Step A4: Repeat step A2 three times, and use high performance liquid chromatography (HPLC) to determine the concentration of THM in the three mixed solutions, and take the average value.
[0088] Test results such as Figure 2 As shown, it can be seen that the THM removal rate increases with the increase of PMS oxidant dosage. When the PMS oxidant dosage is greater than 1.2 mg / L, the THM removal rate reaches 100% within 60 min.
[0089] Test Example 3
[0090] The effect of environmental pH on THM removal rate was investigated.
[0091] Test method:
[0092] Step A1: prepare a THM stock solution with a concentration of 200 ppm using deionized water, take 10 ml of the THM stock solution into a 250 ml beaker, add 90 ml of deionized water, and stir and dilute to obtain a THM solution with a concentration of 20 ppm;
[0093] Step A2: at room temperature, adjust the pH, place the beaker on a magnetic stirrer, add 0.75 mg of the ZnFeBC catalyst of Example 1 and 0.12 mg of the PMS oxidant to the THM solution, stir evenly, and degrade the THM in the THM solution;
[0094] Wherein, the pH is 3, 5, 7, 9, and 11 respectively;
[0095] Step A3: Starting from the moment when the ZnFeBC catalyst and the PMS oxidant are added, within a given reaction interval (0 min, 5 min, 10 min, 20 min, 30 min, 60 min), 0.3 mL of the THM solution is transferred into a small centrifuge tube, filtered through a 0.22 um filter membrane, and then 100 ul is transferred from the small centrifuge tube into a sample injection vial using a 100 ul pipette, and immediately quenched with 0.1 ml of methanol, and finally 0.8 ml of deionized water is added, vortexed, and a mixed solution is obtained;
[0096] Step A4: Repeat step A2 three times, and use high performance liquid chromatography (HPLC) to determine the concentration of THM in the three mixed solutions, and take the average value.
[0097] The test results are as follows Figure 3 As shown, the THM removal rate is optimal at pH = 7, and the ZnFeBC catalyst also has good catalytic performance at other pH values.
[0098] Test Example 4
[0099] The effects of the catalysts of Example 1 and Examples 3-4 on the degradation of thiamethoxam pollutants in water were tested.
[0100] Test method:
[0101] Step A1: prepare a THM stock solution with a concentration of 200 ppm using deionized water, take 10 ml of the THM stock solution into a 250 ml beaker, add 90 ml of deionized water, and stir and dilute to obtain a THM solution with a concentration of 20 ppm;
[0102] Step A2: at room temperature and pH=7, place a beaker on a magnetic stirrer, add 0.75 mg of the ZnFeBC catalyst of Example 1 and Example 3-4 to the THM solution, and add 0.12 mg of the PMS oxidant to the ZnFeBC catalyst of Example 1 and Example 3-4, respectively, and stir evenly to degrade the THM in the THM solution;
[0103] Step A3: Starting from the moment when the catalyst and PMS oxidant are added, within a given reaction interval (0 min, 5 min, 10 min, 20 min, 30 min, 60 min), 0.3 mL of THM solution is transferred to a small centrifuge tube, filtered through a 0.22 um filter membrane, and then 100 ul is transferred from the small centrifuge tube to an injection vial using a 100 ul pipette, and immediately quenched with 0.1 ml of methanol, and finally 0.8 ml of deionized water is added, vortexed, and a mixed solution is obtained;
[0104] Step A4: Repeat step A2 three times, and use high performance liquid chromatography (HPLC) to determine the concentration of THM in the three mixed solutions, and take the average value.
[0105] Test results such as Figure 4 As shown, it can be seen that with the increase of calcination temperature, the catalytic performance of biochar is further improved. When calcined at 700℃, ZnFeBC has the best effect on catalyzing PMS to degrade THM.
[0106] Test Example 5
[0107] The effects of the catalysts of Examples 1-2 and Comparative Examples 1-2 on the degradation of thiamethoxam pollutants in water were tested.
[0108] Test method:
[0109] Step A1: prepare a THM stock solution with a concentration of 200 ppm using deionized water, take 10 ml of the THM stock solution into a 250 ml beaker, add 90 ml of deionized water, and stir and dilute to obtain a THM solution with a concentration of 20 ppm;
[0110] Step A2: at room temperature and pH=7, place a beaker on a magnetic stirrer, add 0.75 mg of the catalyst of Example 1-2 and Comparative Example 1-2 to the THM solution, and add 0.12 mg of PMS oxidant, stir evenly, and degrade THM in the THM solution;
[0111] Step A3: Starting from the moment when the catalyst and PMS oxidant are added, within a given reaction interval (0 min, 5 min, 10 min, 20 min, 30 min, 60 min), 0.3 mL of THM solution is transferred to a small centrifuge tube, filtered through a 0.22 um filter membrane, and then 100 ul is transferred from the small centrifuge tube to an injection vial using a 100 ul pipette, and immediately quenched with 0.1 ml of methanol, and finally 0.8 ml of deionized water is added, vortexed, and a mixed solution is obtained;
[0112] Step A4: Repeat step A2 three times, and use high performance liquid chromatography (HPLC) to determine the concentration of THM in the three mixed solutions, and take the average value.
[0113] The test results are as follows Figure 5 As shown, it can be seen that the effect of biochar ZnFeBC modified by ZnCl2 and K2FeO4 in catalyzing PMS to degrade THM is significantly better than that of ZnBC and BC, and when ZnFeBC is prepared with a mass ratio of 1:1:2 (ZnCl2:K2FeO4:cow dung), the effect of catalyzing PMS to degrade THM is the best.
[0114] Test Example 6
[0115] The effects of the catalysts of Example 1 and Comparative Examples 1-3 on the degradation of thiamethoxam pollutants in water were tested.
[0116] Test method:
[0117] Step A1: prepare a THM stock solution with a concentration of 200 ppm using deionized water, take 10 ml of the THM stock solution into a 250 ml beaker, add 90 ml of deionized water, and stir and dilute to obtain a THM solution with a concentration of 20 ppm;
[0118] Step A2: at room temperature and pH=7, place a beaker on a magnetic stirrer, add 0.75 mg of the ZnFeBC catalyst of Example 1 and the catalysts of Comparative Examples 1-3 to the THM solution, respectively, and add 0.12 mg of the PMS oxidant, stir evenly, and degrade the THM in the THM solution;
[0119] Step A3: Starting from the moment when the catalyst and PMS oxidant are added, within a given reaction interval (0 min, 5 min, 10 min, 20 min, 30 min, 60 min), 0.3 mL of THM solution is transferred to a small centrifuge tube, filtered through a 0.22 um filter membrane, and then 100 ul is transferred from the small centrifuge tube to an injection vial using a 100 ul pipette, and immediately quenched with 0.1 ml of methanol, and finally 0.8 ml of deionized water is added, vortexed, and a mixed solution is obtained;
[0120] Step A4: Repeat step A2 three times, and use high performance liquid chromatography (HPLC) to determine the concentration of THM in the three mixed solutions, and take the average value.
[0121] The test results are as follows Figure 6 As shown, it can be seen that the catalytic performance of the ZnFeBC catalyst of the present invention is significantly better than that of the BC catalyst of Comparative Example 1, the ZnBC catalyst of Comparative Example 2 and the FeBC catalyst of Comparative Example 3, and the THM removal rate reaches 100%. The results show that the catalytic performance of the bimetallic modified biochar is significantly stronger than that of the unmodified BC and the single metal-loaded ZnBC and FeBC, and the two metals synergistically promote the activation of peroxymonosulfate, so that the degradation of pollutants has a better technical effect. Fig. 9 The ZnFeBC catalyst of Example 1 (respectively doped with Fe 0 and Fe3O4) with PMS. Table 1 shows the bond length analysis of the metal species doped on the ZnFeBC surface on the PMS atoms. It can be seen that the Fe 0 The three Fe atoms on the ZnFeBC catalyst react with one S and two O atoms of PMS respectively, while the Fe3O4 on the ZnFeBC catalyst reacts with one oxygen atom of PMS, which increases the SO bond and OO bond of PMS and makes it easier to generate free radicals with strong oxidizing properties.
[0122] Table 1 Effect of metal species doped on the surface of ZnFeBC catalyst on the bond lengths between atoms of PMS
[0123] Key length OO S-O1 S-O2 S-O3 S-O4 PMS original bond length 1.45 1.46 1.47 1.49 1.70 <![CDATA[Fe 0 ]]> 1.54 1.58 1.64 1.56 1.74 <![CDATA[Fe2O3]]> 1.47 1.46 1.52 1.49 1.69 <![CDATA[Fe3O4]]> 1.49 1.46 1.47 1.55 1.68
[0124] Test Example 7
[0125] The catalysts of Example 1 and Comparative Examples 1-2 were characterized by XRD and analyzed by FTIR spectra.
[0126] Figure 7 Comparison of the XRD patterns of ZnFeBC catalyst, BC catalyst and ZnFeBC catalyst shows that the surface of ZnFeBC catalyst is loaded with ZnO and Fe, providing abundant active sites, and the surface of ZnBC catalyst is loaded with ZnO.
[0127] Figure 8 The FTIR images of ZnFeBC catalyst, BC catalyst and ZnFeBC catalyst are compared. It can be seen that compared with BC catalyst and ZnBC catalyst, the surface of ZnFeBC catalyst contains abundant oxygen-containing functional groups. In order to explore the mechanism of ZnFeBC activating PMS to degrade THM, DFT calculation was carried out. From the molecular level, the Fe loaded on the surface of ZnFeBC 0and Fe3O4 are the main active sites, which greatly improves the catalytic performance of the catalyst.
[0128] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0129] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A bimetallic doped biochar catalyst, characterized in that: The bimetallic doped biochar catalyst comprises biochar having a porous structure, ZnO, Fe 0 , Fe2O3 and Fe3O4.
2. The bimetallic doped biochar catalyst according to claim 1, characterized in that: The specific surface area of the bimetallic doped biochar catalyst is 130-150m 2 / g.
3. The bimetallic doped biochar catalyst according to claim 1, characterized in that: The pore size of the biochar is 10-14 nm.
4. The bimetallic doped biochar catalyst according to claim 1, characterized in that: The raw material of the biochar is livestock manure.
5. The method for preparing the bimetallic doped biochar catalyst according to any one of claims 1 to 4, characterized in that: The steps include: S1, adding livestock manure, zinc salt and K2FeO4 into water, heating, stirring and grinding to obtain a mixed powder; S2. Under the protection of an inert gas, the mixed powder is carbonized and purified to obtain a bimetallic doped biochar catalyst.
6. The method for preparing a bimetallic doped biochar catalyst according to claim 5, characterized in that: In step S1, the heating temperature is 75-85°C.
7. The method for preparing a bimetallic doped biochar catalyst according to claim 5, characterized in that: In step S2, the temperature of the carbonization treatment is 500-700°C and the time is 1.5-4h.
8. The method for preparing a bimetallic doped biochar catalyst according to claim 7, characterized in that: In step S2, the temperature rise rate is 3-7°C / min.
9. The method for preparing a bimetallic doped biochar catalyst according to claim 5, characterized in that: In step S2, a sulfuric acid solution is also required to absorb tail gas during the carbonization process; Wherein, the volume ratio of sulfuric acid to water in the sulfuric acid solution is 1-2:3-5.
10. Use of the bimetallic doped biochar catalyst according to any one of claims 1 to 4 in water treatment.
Citation Information
Patent Citations
Method by using green bio-charcoal for high-effectively catalytically degrading soluble organic substance NOM in environment
CN109201087A
Preparation method and application of biomass porous carbon material
CN111204755A
Preparation method and application of sludge-based activated carbon material for adsorbing phenol in aqueous solution
CN116459793A