Catalyst for preparing methacrylic acid by isobutene one-step oxidation method and method for preparing methacrylic acid
By using the catalysts of Mo7V3P0.3Ce0.3O27 and K0.6CsWH1.4PMo11VO40, the problem of high conversion rate but low selectivity in the one-step oxidation method is solved, and efficient and green methacrylic preparation is achieved, reducing the complexity of the reaction process and equipment costs.
Patent Information
- Application Number
- CN202411029162.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing one-step oxidation method of isobutene to prepare methacrylic acid has a high conversion rate but low selectivity, and the preparation process is not green enough, which has problems such as environmental pollution and high equipment requirements.
The catalysts of composite metal oxide component Mo7V3P0.3Ce0.3O27 and heteropolyacid component K0.6CsWH1.4PMo11VO40 are used to increase the proportion of strong acid sites in the catalyst by modifying the heteropolyacid catalyst, and the oxidation capacity is improved by combining Ce element. The direct oxidation of isobutene to methacrylic acid is achieved by realizing a one-step process.
It improves the selectivity and conversion rate of methacrylic acid, reduces the complexity of reaction process and equipment costs, and realizes green and environmentally friendly catalyst preparation.
Smart Images

Figure CN118874504A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical synthesis, and particularly relates to a catalyst for preparing methacrylic acid by a one-step oxidation process of isobutylene and a method for preparing methacrylic acid. Background Art
[0002] Methacrylic acid is an important organic synthetic raw material and chemical intermediate, widely used in chemical products such as synthetic resins, polymers, coatings and adhesives.
[0003] At present, the production method of preparing methacrylic acid by oxidation of isobutylene mostly includes two steps: first, oxidizing isobutylene to methacrolein, often using Mo-Bi or Mo-V composite metal oxide catalysts; then oxidizing methacrolein to methacrylic acid, often using Mo-P heteropoly acid and other oxidants as catalysis. For the first step reaction, patent document CN113710362 B uses Mo, Bi, and Fe as the main active components, and Co, Ni, Cs, and W as co-catalysts to prepare methacrolein by catalytic reaction in a tubular fixed bed reactor. The conversion rate of isobutylene can be as high as 95.4%, the selectivity of methacrolein is 85.7%, and the selectivity of methacrylic acid is low, only 4.2%. Patent document CN 114917924 B prepares a supported catalyst, whose main active component is Au, and the carrier is a composite metal oxide containing components such as Mo, Bi, and Co. The catalyst reduces the temperature of the oxidation reaction by introducing a small amount of gold element during the preparation process, thereby improving the selectivity of selective oxidation of isobutylene to prepare methacrolein. For the second step reaction, patent document CN 116196955 A uses a heteropoly acid catalyst with Mo, V, P, and Ag as the main active components, adds a thermal conductor to shape the catalyst, and adopts microwave reaction and step-by-step calcination methods in the catalyst preparation process to obtain a higher methacrolein conversion rate and methacrylic acid selectivity under milder reaction conditions. Patent document CN 114849747 B adds K, Cs, and NH4 to the Mo-P system heteropoly acid as counter cations, and uses kaolin as a catalyst carrier to improve the acidity of the catalyst and the selectivity and thermal stability of methacrylic acid. After reading some patent documents, it is found that the method for preparing methacrylic acid mostly adopts a two-step method, and the reaction is carried out in two different catalyst systems and two-stage reactors.
[0004] At present, there are also a small number of reports on catalyst systems for preparing methacrylic acid by one-step oxidation. Patent document CN 114849740A uses a composite oxide catalyst with Mo and V as the main active components, and uses Te and Cs as co-catalysts to improve the selectivity of isobutylene selective oxidation to methacrylic acid. The conversion rate of isobutylene is 90%, and the selectivity of methacrylic acid is as high as 70%. However, the preparation process of the catalyst is not green enough, and expensive and explosive reagents are used. Patent document CN 114471530 A, Mo-Bi composite oxide is dispersed in a surfactant and compounded with a Mo-P-based heteropoly compound containing a silicon dioxide precursor to form a two-component catalyst, improve the thermal stability of the heteropoly acid catalyst, the conversion rate of isobutylene is 97.0%, and the selectivity of methacrylic acid is as high as 78.4%, but the precursor of its main component Bi, bismuth nitrate, is insoluble in water, so nitric acid solution is used as a solvent in the preparation process, which is harmful to the environment and has high requirements for equipment. At present, in the research on catalysts for preparing methacrylic acid by one-step oxidation of isobutylene, although the conversion rate of isobutylene is high, its selectivity for the target product methacrylic acid is not high. Therefore, it is urgent to develop a one-step oxidation method for preparing methacrylic acid using isobutylene as a raw material, which is pollution-free and harmless, has high atomic utilization rate, and high selectivity for methacrylic acid, which can greatly reduce the complexity of the reaction process, reduce the initial equipment investment, and reduce the production cost. Summary of the invention
[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a catalyst for preparing methacrylic acid by one-step oxidation of isobutylene and a method for preparing methacrylic acid.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene, comprising a composite metal oxide component and a heteropolyacid component; the composite metal oxide component is composed of Mo7V3P 0.3 Ce a O 27 , wherein a represents the number of atoms of Ce element, and the value is 0.05-0.1; the composition of the heteropoly acid component is K 0.6 Wlq 1.4 PMo 11 VO 40 .
[0008] On the basis of the above scheme, the mass ratio of the composite metal oxide component to the heteropolyacid component is 3:2-1:4.
[0009] The preparation method of the catalyst for preparing methacrylic acid by the one-step oxidation of isobutylene comprises the following steps:
[0010] The composite metal oxide component aqueous solution is added to the solution of the heteropolyacid component, stirred, the solvent is evaporated, and dried to obtain a yellow solid; the solid is ground into powder, and calcined at 300-450° C. for 5-12 hours with a heating rate of 5° C. / min to obtain a catalyst for preparing methacrylic acid by a one-step oxidation method of isobutylene.
[0011] On the basis of the above scheme, the composite metal oxide component is prepared by the following method:
[0012] ① Add deionized water to a mixture of ammonium heptamolybdate and ammonium metavanadate in a mass ratio of 1:0.4-1:0.09, and stir and dissolve at 60-90° C. for 30-60 min to obtain a mixed solution I;
[0013] ② Adding ammonium dihydrogen phosphate to the mixed solution I to obtain a mixed solution II;
[0014] ③ Dissolving cerium nitrate hexahydrate in deionized water to obtain a mixed solution III;
[0015] ④ Add mixed solution III to mixed solution II, stir for 120-130 min, raise the temperature to 85-95°C and continue stirring until the reaction solution is evaporated to dryness, and dry the obtained solid material at 80-120°C for 10-12h;
[0016] ⑤ Grind the solid material dried in step ④, and finally calcine the solid powder at a temperature of 500-600° C. for 2-5 hours and a heating rate of 5° C. / min to obtain the composite metal oxide component.
[0017] On the basis of the above scheme, the solution of the heteropolyacid component is prepared by the following method:
[0018] ① Add deionized water to a mixture of MoO3 and V2O5 in a mass ratio of 1.0:0.06-1.0:0.05, heat and stir at 60-80°C for 20-30 minutes to obtain solution IV;
[0019] ② Add 85% H3PO4 aqueous solution dropwise to solution IV, heat at 90°C, stir and reflux for 5-7h until an orange-red transparent solution V is obtained, then stop refluxing;
[0020] ③ The transparent orange-red liquid V obtained above was stirred and evaporated to dryness, and then dried at 80-120°C for 10-12h to obtain H4PMo 11 VO 40 ;
[0021] ④ Take H4PMo 11 VO 40 Dissolve in deionized water and stir at 60-80°C to obtain solution VI;
[0022] ⑤ Dissolve CsOH·H2O, KOH and Na2WO4·2H2O in water, slowly add to solution VI and stir for 10 minutes; stir the obtained suspension at 80°C for 3 hours to obtain solution VII, that is, a solution of the heteropolyacid component.
[0023] On the basis of the above scheme, the mass ratio of ammonium heptamolybdate to ammonium dihydrogen phosphate is 1.0:0.5-1.0:0.02; the mass ratio of ammonium heptamolybdate to cerium nitrate hexahydrate is 1.0:0.1-1.0:0.017.
[0024] The catalyst prepared by the method is used in preparing methacrylic acid by one-step oxidation of isobutylene.
[0025] A method for preparing methacrylic acid by one-step oxidation of isobutylene, comprising the following steps:
[0026] The catalyst prepared by the above method was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm, and quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst; the reaction tube was loaded into a tubular furnace reactor, and the catalyst bed temperature was set to 360-440°C, the pressure was normal pressure, the feed volume ratio of isobutylene and air was 1:25, and the feed space velocity was 660-1320h -1 .
[0027] Based on the above scheme, the catalyst bed temperature is 400°C.
[0028] Based on the above scheme, the feed space velocity is 1320h -1 .
[0029] On the basis of the above scheme, the mass ratio of the composite metal oxide component to the heteropoly acid component in the catalyst is 1:1; the composite metal oxide component is Mo7V3P 0.3 Ce 0.075 O 27 .
[0030] Advantages of the technical solution of the present invention:
[0031] The invention provides a composite catalyst for preparing methacrylic acid by one-step selective oxidation of isobutylene. The composite catalyst increases the proportion of strong acid sites in the catalyst by combining Mo-V series oxides with a modified heteropolyacid catalyst under green and environmentally friendly conditions, is beneficial to the selectivity of MAA, and can improve the yield of MAA while maintaining a high conversion rate of isobutylene.
[0032] The catalyst of the present invention has two active components and can directly oxidize isobutylene into methacrylic acid in one step. Compared with the single-component catalyst in the prior art, the two-component composite structure has good thermal stability, high conversion rate and good methacrylic acid selectivity.
[0033] The catalyst of the present invention does not require multi-stage oxidation reactions and can directly oxidize isobutylene into methacrylic acid in one step in a reactor. The reaction cycle and process of this method are short, and the preparation method of the catalyst is simple.
[0034] The method for preparing methacrylic acid by one-step oxidation using isobutylene as a raw material by using the catalyst of the present invention reduces the complexity of the reaction process and reduces the initial equipment cost investment. For the composite catalyst, the asymmetric lattice oxygen is combined with a moderately acidic heteropolyacid catalyst, Ce can improve the oxidation ability of the active Mo species, promote oxygen activation to form lattice oxygen, and increase the proportion of medium and strong acid sites of the catalyst, while maintaining a high conversion rate of isobutylene, the selectivity of methacrylic acid is improved, and isobutylene is efficiently oxidized to methacrylic acid in one step. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Mo7V3P 0.3 Ce 0.1 O 27 Scanning electron microscopy image of / KCsWPAV composite catalyst;
[0036] Figure 2 Mo7V3P 0.3 Ce 0.1 O 27 X-ray diffraction pattern of / KCsWPAV composite catalyst;
[0037] Figure 3 Mo7V3P 0.3 Ce 0.1 O 27 Infrared spectrum of / KCsWPAV composite catalyst;
[0038] Figure 4 Schematic diagram of the one-step oxidation reaction apparatus for isobutylene. DETAILED DESCRIPTION
[0039] The terms used in the present invention, unless otherwise specified, generally have the meanings commonly understood by those of ordinary skill in the art. The present invention will be further described in detail below in conjunction with specific examples and with reference to data. The following examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention in any way.
[0040] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.
[0041] In the following examples, the crystal structure characteristics of the composite catalyst were measured using a Rigaku D / Max 2500 XRD powder tester and a Nicolet 8700 Fourier transform infrared (FT-IR) spectrometer manufactured in the United States.
[0042] The present invention adopts a chromatograph to perform online analysis on the product, and the conversion rate of isobutylene and the selectivity of methacrylic acid are used as performance indicators for evaluating the catalyst, which are defined as follows:
[0043] Isobutylene conversion = (number of moles of i-C4H8 reacted / number of moles of i-C4H8 supplied as raw material) × 100%
[0044] MAA selectivity = (number of moles of MAA produced / number of moles of i-C4H8 reacted) × 100%
[0045] Example 1
[0046] A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene is prepared by the following method:
[0047] (1) Preparation of Mo-VP catalyst
[0048] ① Weigh 6.180 g of ammonium heptamolybdate and 1.755 g of ammonium metavanadate into a three-necked flask, add 50 mL of deionized water, place the three-necked flask in a constant temperature magnetic stirrer, stir at 80°C for about 30 min, and wait until the solid matter is completely dissolved to obtain a mixed solution I.
[0049] ② Weigh 0.173 g of ammonium dihydrogen phosphate and add it to mixed solution I to obtain mixed solution II;
[0050] ③ Weigh 0.217 g of cerium nitrate hexahydrate and dissolve it in 5 mL of deionized water, and dissolve it in an ultrasonic cleaner to obtain a mixed solution III.
[0051] ④ Add mixed solution III to mixed solution II, continue stirring at 80°C for 2h, then increase the water bath temperature to 90°C and continue stirring until the reaction liquid in the container is evaporated to dryness. Place the obtained solid material in an electric constant temperature blast drying oven and dry it overnight at a drying temperature of 80°C.
[0052] ⑤ Grind the dried solid using a ceramic mortar, and finally place the solid powder in a ceramic boat and calcine it in a tube furnace. The calcination procedure is calcination at 600°C for 4 hours with a heating rate of 5°C / min. The calcined solid powder is the Mo-VP catalyst, with a composition of Mo7V3P 0.3 Ce 0.1 O 27 .
[0053] (2)Mo7V3P 0.3 Ce 0.1 O 27 Preparation of KCsWPAV / KCs composite catalyst
[0054] ① Weigh 14.400g MoO3 and 0.825g V2O5 respectively and add them to a 500mL three-necked flask, add 250mL deionized water, put in a magnetic bar, place the three-necked flask in a constant temperature heating and stirring water bath, plug the left and right ports with stoppers, connect the middle port to a serpentine condenser, connect the condenser to tap water, turn on heating and stirring for 20min to obtain solution IV, and set the heating temperature to 80℃;
[0055] ②Use a pipette to evenly add 1.048 g of 85% H3PO4 diluted with 10 mL of deionized water into the three-necked flask dropwise, plug the flask, increase the temperature to 90°C, heat and stir under reflux for 5 h until an orange-red transparent solution V is obtained, then stop the reflux.
[0056] ③ Pour the above-obtained transparent orange-red liquid into a beaker, wash the three-necked flask and pour the liquid into the beaker, put in a magnet, stir and evaporate to dryness in a constant temperature water bath at 80°C, take it out and place it in a constant temperature blast drying oven at 80°C to dry for 12 hours, and finally obtain bright yellow solid H4PMo 11 VO 40 , abbreviated as HPAV.
[0057] ④ Take 3 g of HPAV solid powder and dissolve it in 100 mL of deionized water and stir at 80°C for 20 min to obtain solution VI.
[0058] ⑤ Then 0.282g of CsOH·H2O, 0.056g of KOH and 0.555g of Na2WO4·2H2O were dissolved in 10mL of water, slowly added to solution VI and stirred for 10min. After that, the suspension was vigorously stirred at 80℃ for 3h to obtain solution VII. The heteropoly acid component is K 0.6 Wlq 1.4 PMo 11 VO 40 , the heteropolyacid component remains unchanged and is abbreviated as KCsWPAV.
[0059] ⑥Weigh 3.000g Mo7V3P0.3 Ce 0.1 O 27 The catalyst was dissolved in 10 mL of deionized water to obtain solution VIII, and solution VIII was added to solution VII, and then continued to stir evenly. The solvent was evaporated by rotary evaporation, and the obtained solid material was dried in an oven at 80° C. overnight to obtain a yellow solid.
[0060] ⑦ Grind the dried solid using a ceramic mortar, and finally place the solid powder in a ceramic boat and calcine it in a tube furnace. The calcination procedure is calcination at 350℃ for 7h, with a heating rate of 5℃ / min. The solid powder after calcination is Mo7V3P 0.3 Ce 0.1 O 27 / KCsWPAV composite catalyst.
[0061] Two active components Mo7V3P in the catalyst preparation process 0.3 Ce 0.1 O 27 The mass ratio with KCsWPAV is 1:1.
[0062] Mo7V3P prepared by the above method 0.3 Ce 0.1 O 27 The / KCsWPAV composite catalyst was observed by scanning electron microscope. Figure 1 As shown, Figure 1 The scale bar is 200 nm. The surface of the composite catalyst is dispersed with long flakes and spherical columns. 0.3 Ce 0.1 O 27 The / KCsWPAV composite catalyst has the performance characteristics of Mo-V based composite oxide catalyst and heteropolyacid catalyst.
[0063] Mo7V3P 0.3 Ce 0.1 O 27 X-ray diffraction analysis of KCsWPAV composite catalyst Figure 2 As shown, some prominent diffraction peaks correspond to Mo6V9O in the orthorhombic system. 40 The characteristic peaks of the crystal plane indicate that a new material structure has been formed between Mo and V. Based on the structure of Mo6V9O4 determined by powder neutron diffraction, the existence of Mo-OV can be preliminarily inferred indirectly. The diffraction peaks at 2θ=10.56°, 19.9° and 26.14° are similar to those of Keggin structure heteropoly acid H4PMo 11 VO 40 The results are completely consistent, indicating that the finished catalyst has a stable heteropolyacid structure.
[0064] Mo7V3P0.3 Ce 0.1 O 27 Infrared spectrum analysis of / KCsWPAV composite catalyst Figure 3 As shown, at 967cm -1 The peak at 592 cm corresponds to the Mo=O bond. -1 The peak at 500-2000cm corresponds to the VOV bond, which is characteristic of metal oxides. -1 The catalyst shows the typical IR absorption bands of Keggin structure, which correspond to the P=O bond in the catalytic center, the Mo=O terminal oxygen bond, and the Mo-O b -Mo bridge oxygen bond and intergroup Mo-O c -Mo bridge oxygen bond, these characteristic peaks further indicate that the composite catalyst has the characteristics of Keggin-type structure.
[0065] Example 2
[0066] A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene is prepared by the following method:
[0067] Except for the following steps, the remaining steps are the same as those in Example 1.
[0068] (2)Mo7V3P 0.3 Ce 0.1 O 27 Preparation of KCsWPAV / KCs composite catalyst
[0069] ⑥Weigh 4.500g Mo7V3P 0.3 Ce 0.1 O 27 The catalyst was dissolved in 10 mL of deionized water to obtain solution VIII, and solution VIII was added to solution VII, and then continued to stir evenly. The solvent was evaporated by rotary evaporation, and the obtained solid material was dried in an oven at 80° C. overnight to obtain a yellow solid.
[0070] Two active components Mo7V3P in the catalyst preparation process 0.3 Ce 0.1 O 27 The mass ratio with KCsWPAV is 3:2.
[0071] The catalyst component prepared by the above method is Mo7V3P 0.3 Ce 0.1 O 27 / KCsWPAV.
[0072] Example 3
[0073] A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene is prepared by the following method:
[0074] Except for the following steps, the remaining steps are the same as those in Example 1.
[0075] (2)Mo7V3P 0.3 Ce 0.1 O 27 Preparation of KCsWPAV / KCs composite catalyst
[0076] ⑥Weigh 2.000g Mo7V3P 0.3 Ce 0.1 O 27 The catalyst was dissolved in 10 mL of deionized water to obtain solution VIII, and solution VIII was added to solution VII, and then continued to stir evenly. The solvent was evaporated by rotary evaporation, and the obtained solid material was dried in an oven at 80° C. overnight to obtain a yellow solid.
[0077] Two active components Mo7V3P in the catalyst preparation process 0.3 Ce 0.1 O 27 The mass ratio with KCsWPAV is 2:3.
[0078] The catalyst component prepared by the above method is Mo7V3P 0.3 Ce 0.1 O 27 / KCsWPAV.
[0079] Example 4
[0080] A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene is prepared by the following method:
[0081] Except for the following steps, the remaining steps are the same as those in Example 1.
[0082] (2)Mo7V3P 0.3 Ce 0.1 O 27 Preparation of KCsWPAV / KCs composite catalyst
[0083] ⑥Weigh 1.280g Mo7V3P 0.3 Ce 0.1 O 27 The catalyst was dissolved in 10 mL of deionized water to obtain solution VIII, and solution VIII was added to solution VII, and then continued to stir evenly. The solvent was evaporated by rotary evaporation, and the obtained solid material was dried in an oven at 80° C. overnight to obtain a yellow solid.
[0084] Two active components Mo7V3P in the catalyst preparation process 0.3 Ce 0.1 O 27 The mass ratio with KCsWPAV is 3:7.
[0085] The catalyst component prepared by the above method is Mo7V3P 0.3 Ce 0.1 O 27 / KCsWPAV.
[0086] Example 5
[0087] A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene is prepared by the following method:
[0088] Except for the following steps, the remaining steps are the same as those in Example 1.
[0089] (2)Mo7V3P 0.3 Ce 0.1 O 27 Preparation of KCsWPAV / KCs composite catalyst
[0090] ⑥Weigh 0.750g Mo7V3P 0.3 Ce 0.1 O 27 The catalyst was dissolved in 10 mL of deionized water to obtain solution VIII, and solution VIII was added to solution VII, and then continued to stir evenly. The solvent was evaporated by rotary evaporation, and the obtained solid material was dried in an oven at 80° C. overnight to obtain a yellow solid.
[0091] Two active components Mo7V3P in the catalyst preparation process 0.3 Ce 0.1 O 27 The mass ratio with KCsWPAV is 1:4.
[0092] The catalyst component prepared by the above method is Mo7V3P 0.3 Ce 0.1 O 27 / KCsWPAV.
[0093] Example 6
[0094] A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene is prepared by the following method:
[0095] Except for the following steps, the remaining steps are the same as those in Example 1.
[0096] (1) Preparation of Mo-VP catalyst
[0097] ③ Weigh 0.109 g of cerium nitrate hexahydrate and dissolve it in 5 mL of deionized water, and dissolve it in an ultrasonic cleaner to obtain a mixed solution III.
[0098] The catalyst component prepared by the above method is Mo7V3P 0.3 Ce 0.05 O 27 / KCsWPAV.
[0099] Example 7
[0100] A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene is prepared by the following method:
[0101] Except for the following steps, the remaining steps are the same as those in Example 1.
[0102] (1) Preparation of Mo-VP catalyst
[0103] ③ Weigh 0.163 g of cerium nitrate hexahydrate and dissolve it in 5 mL of deionized water, and dissolve it in an ultrasonic cleaner to obtain a mixed solution III.
[0104] The catalyst component prepared by the above method is Mo7V3P 0.3 Ce 0.075 O 27 / KCsWPAV.
[0105] Example 8
[0106] A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene is prepared by the following method:
[0107] Except for the following steps, the remaining steps are the same as those in Example 1.
[0108] (1) Preparation of Mo-VP catalyst
[0109] ③ Weigh 0.184 g of cerium nitrate hexahydrate and dissolve it in 5 mL of deionized water, and dissolve it in an ultrasonic cleaner to obtain a mixed solution III.
[0110] The catalyst component prepared by the above method is Mo7V3P 0.3 Ce 0.085 O 27 / KCsWPAV.
[0111] Example 9
[0112] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0113] 1.000 g of the composite catalyst prepared by the method of Example 1 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 400°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 90% and the selectivity of methacrylic acid was 50%.
[0114] The above reaction process can be carried out using existing equipment or by using Figure 4 The device shown:
[0115] Isobutylene and air flow out of the gas cylinder, and the gas flow is controlled by adjusting the flow meter through the controller. After mixing, they enter the tubular furnace reactor equipped with a catalyst to generate gas phase products containing methacrolein and methacrylic acid. After condensation, the products enter the capture bottle filled with ethanol for collection, and the gas components are collected by a gas sampling bag. The whole process is continuous.
[0116] Example 10
[0117] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0118] 1.000 g of the composite catalyst prepared by the method of Example 1 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 360°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 93%, and the selectivity of methacrylic acid was 25.4%.
[0119] Embodiment 11
[0120] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0121] 1.000 g of the composite catalyst prepared by the method of Example 1 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 380°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 90%, and the selectivity of methacrylic acid was 30.9%.
[0122] Example 12
[0123] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0124] 1.000 g of the composite catalyst prepared by the method of Example 1 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 420°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 87% and the selectivity of methacrylic acid was 45.4%.
[0125] Example 13
[0126] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0127] 1.000 g of the composite catalyst prepared by the method of Example 1 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 440°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 88% and the selectivity of methacrylic acid was 35%.
[0128] Embodiment 14
[0129] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0130] 1.000 g of the composite catalyst prepared by the method of Example 2 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 400°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 91%, and the selectivity of methacrylic acid was 43.6%.
[0131] Embodiment 15
[0132] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0133] 1.000 g of the composite catalyst prepared by the method of Example 3 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 400°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 90%, and the selectivity of methacrylic acid was 25.4%.
[0134] Example 16
[0135] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0136] 1.000 g of the composite catalyst prepared by the method of Example 4 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 400°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 88%, and the selectivity of methacrylic acid was 40.9%.
[0137] Embodiment 17
[0138] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0139] 1.000 g of the composite catalyst prepared by the method of Example 5 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 400°C, the pressure was normal pressure, the feed volume ratio of isobutylene and air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 85%, and the selectivity of methacrylic acid was 31.7%.
[0140] Embodiment 18
[0141] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0142] 1.000 g of the composite catalyst prepared by the method of Example 6 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 400°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 87% and the selectivity of methacrylic acid was 0%.
[0143] Embodiment 19
[0144] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0145] 1.000 g of the composite catalyst prepared by the method of Example 7 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 400°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 93% and the selectivity of methacrylic acid was 80.5%.
[0146] Embodiment 20
[0147] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0148] 1.000 g of the composite catalyst prepared by the method of Example 8 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 400°C, the pressure was normal pressure, the feed volume ratio of isobutylene and air was 1:25, and the feed space velocity was 1320 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 89% and the selectivity of methacrylic acid was 46.5%.
[0149] Embodiment 21
[0150] The method for preparing methacrylic acid by one-step oxidation of isobutylene comprises the following steps:
[0151] 1.000 g of the composite catalyst prepared by the method of Example 1 was loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm. The reaction tube was loaded into a tubular furnace reactor. A certain amount of quartz wool was placed in the non-constant temperature zone to fill the two ends of the catalyst to ensure that the gas reactants pass through the catalyst bed evenly. The catalyst bed temperature was set to 400°C, the pressure was normal pressure, the feed volume ratio of isobutylene to air was 1:25, and the feed space velocity was 660 h -1 After running the reaction for 1 hour, the catalyst was sampled and analyzed, and the conversion rate of isobutylene was 90%, and the selectivity of methacrylic acid was 50.7%.
[0152] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A catalyst for preparing methacrylic acid by one-step oxidation of isobutylene, characterized in that: It comprises a composite metal oxide component and a heteropoly acid component; the composite metal oxide component is composed of Mo7V3P 0.3 Ce a O 27 , wherein a represents the number of atoms of Ce element, and the value is 0.05-0.1; the composition of the heteropoly acid component is K 0.6 Wlq 1.4 PMo 11 VO 40 .
2. The catalyst for preparing methacrylic acid by one-step oxidation of isobutylene according to claim 1, characterized in that: The mass ratio of the composite metal oxide component to the heteropolyacid component is 3:2-1:
4.
3. The method for preparing a catalyst for preparing methacrylic acid by one-step oxidation of isobutylene according to claim 1 or 2, characterized in that: Here are the steps: The composite metal oxide component aqueous solution is added to the solution of the heteropolyacid component, stirred, the solvent is evaporated, and dried to obtain a yellow solid; the solid is ground into powder, and calcined at 350°C for 7 hours with a heating rate of 5°C / min to obtain a catalyst for preparing methacrylic acid by a one-step oxidation method of isobutylene.
4. The method for preparing a catalyst for preparing methacrylic acid by one-step oxidation of isobutylene according to claim 3, characterized in that: The composite metal oxide component is prepared by the following method: ① Add deionized water to the mixture of ammonium heptamolybdate and ammonium metavanadate, stir and dissolve to obtain a mixed solution I; ② Adding ammonium dihydrogen phosphate to the mixed solution I to obtain a mixed solution II; ③ Dissolving cerium nitrate hexahydrate in deionized water to obtain a mixed solution III; ④ Add the mixed solution III to the mixed solution II, stir, and continue stirring after heating until the reaction solution is evaporated to dryness, and dry the obtained solid matter overnight; ⑤ Grind the solid material dried in step ④, and finally calcine the solid powder at 600° C. for 4 h at a heating rate of 5° C. / min to obtain the composite metal oxide component.
5. The method for preparing a catalyst for preparing methacrylic acid by one-step oxidation of isobutylene according to claim 4, characterized in that: The solution of the heteropolyacid component is prepared by the following method: ① Add deionized water to the mixture of MoO3 and V2O5, heat and stir at 80°C for 20 minutes to obtain solution IV; ② Add 85% H3PO4 aqueous solution dropwise to solution IV, heat at 90°C, stir and reflux for 5 h until an orange-red transparent solution V is obtained, then stop refluxing; ③ The transparent orange-red liquid V obtained above was stirred in a constant temperature water bath at 80°C and evaporated to dryness, and then dried at 80°C for 12h to obtain H4PMo 11 VO 40 ; ④ Take H4PMo 11 VO 40 Dissolve in deionized water and stir at 80 °C for 20 min to obtain solution VI; ⑤ Dissolve CsOH·H2O, KOH and Na2WO4·2H2O in water, slowly add to solution VI and stir for 10 minutes; stir the obtained suspension at 80°C for 3 hours to obtain solution VII, that is, a solution of the heteropolyacid component.
6. Use of the catalyst prepared by the method of claim 5 in the preparation of methacrylic acid by one-step oxidation of isobutylene.
7. A method for preparing methacrylic acid by one-step oxidation of isobutylene, characterized in that: Here are the steps: The catalyst prepared by the method of claim 5 is loaded into the constant temperature zone of a quartz glass reaction tube with an inner diameter of 20 mm, an outer diameter of 25 mm, and a length of 45 cm, and quartz wool is placed in the non-constant temperature zone to fill the two ends of the catalyst; the reaction tube is loaded into a tubular furnace reactor, and the catalyst bed temperature is set to 360-440°C, the pressure is normal pressure, the feed volume ratio of isobutylene and air is 1:25, and the feed space velocity is 660-1320h -1 .
8. The method for preparing methacrylic acid by one-step oxidation of isobutylene according to claim 7, characterized in that: The catalyst bed temperature is 400°C.
9. The method for preparing methacrylic acid by one-step oxidation of isobutylene according to claim 7, characterized in that: The feed space velocity is 1320h -1 .
10. The method for preparing methacrylic acid by one-step oxidation of isobutylene according to any one of claims 7 to 9, characterized in that: The mass ratio of the composite metal oxide component to the heteropoly acid component in the catalyst is 1:1; the composite metal oxide component is Mo7V3P 0.3 Ce 0.075 O 27 .
Citation Information
Patent Citations
Catalyst for production of methacryhi acid and method for production of methacrylic acid
CN1126718A
Composite catalyst for manufacturing methacrylic acid and preparation method thereof
CN114471530A
Process for producing methacrylic acid and catalyst therefor
GB1498595A
Method for producing methacrylic acid
JP2005187463A
Promoted multi-metal oxide catalyst
US20020065431A1