Method for preparing high-quality titanium concentrate from ilmenite flotation concentrate
Through the combination of agents, multiple stirring and ultrasonic screening grading technology, the problems of CaO, SiO2, and Al2O3 impurities in ilmenite are solved, and the preparation of high-quality titanium concentrate is achieved, and the TiO2 grade and processing efficiency of titanium concentrate are improved.
Patent Information
- Application Number
- CN202410973425.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The prior art is difficult to effectively improve the TiO2 grade of titanium concentrate, while reducing the CaO, SiO2, and Al2O3 content in ilmenite flotation concentrate, and the adsorption of flotation agents on the mineral surface leads to flocculation, affecting subsequent processing.
The combination of agents includes sodium carbonate, water glass, etc., through multiple stirring and ultrasonic screening, the sufficient separation of ilmenite and gangue minerals is achieved, the impurity content is reduced, and high-quality titanium concentrate is prepared.
It significantly improves the TiO2 grade of titanium concentrate, reduces the CaO, SiO2 and Al2O3 content, reduces the tailings loss rate, and improves the quality and economic benefits of titanium concentrate.
Smart Images

Figure CN118874689A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a method for preparing high-quality titanium concentrate by utilizing ilmenite flotation concentrate. Background Art
[0002] Titanium is an important rare strategic metal with a series of excellent properties that other metals cannot match, such as high specific strength, light weight, corrosion resistance, shape memory, good ductility and biocompatibility, superconductivity and strong surface decoration. It has a wide range of uses in various fields such as aerospace, petrochemicals, construction, electricity, medical treatment, and sports goods. Titanium is called the "third metal" after iron and aluminum. TiO2 is the best white inorganic pigment and is widely used in coatings, plastics, chemical fibers, rubber, papermaking, printing inks, cosmetics and other industries. The main titanium-containing minerals with industrial value in nature are ilmenite and rutile. The world's titanium resources (in terms of TiO2) exist in the form of ilmenite, accounting for about 93.42%. my country's titanium resources account for 25% of the world's total resources, of which 93% are distributed in the form of primary ilmenite in the vanadium-titanium magnetite in the Panxi area. The development and utilization of Panxi titanium resources is of great significance to my country's national defense construction, industry and economic development.
[0003] Since the early 1980s, my country's Panxi region has been recovering titanium resources from vanadium-titanium magnetite iron tailings. Its process has been reformed from spiral chute re-selection-flotation desulfurization-drying-electrostatic selection of titanium, and now it has been widely used in strong magnetic separation-flotation desulfurization-flotation selection of titanium. At present, the area produces about 80% of the titanium concentrate produced by my country's titanium industry. The TiO2 grade of primary ilmenite concentrate produced from vanadium magnetite in my country is generally 45%-47%. The low TiO2 grade and rich in CaO, SiO2, and Al2O3 have restricted the development of my country's titanium industry chain, making my country's titanium dioxide industry mainly sulfuric acid method and molten salt chlorination, and unable to use boiling chlorination, which affects the competitiveness of my country's titanium industry chain. In actual application, boiling chlorination usually requires CaO≤0.15%, Al2O3≤1.50%, and SiO2≤1.0% in titanium concentrate, especially the strict requirements on CaO content. At the same time, in the process of producing titanium concentrate from vanadium-titanium magnetite ilmenite in my country, flotation agents are added during flotation desulfurization and flotation titanium selection. The flotation agents are adsorbed on the surface of the minerals, causing the ilmenite to form flocs in the slurry, which is not conducive to the subsequent use of other methods to increase the TiO2 grade of the flotation titanium concentrate. The effect of reducing CaO by increasing the number of flotation stages is not obvious and affects the TiO2 recovery rate of the titanium concentrate.
[0004] CN117483097A discloses a low-grade ilmenite beneficiation process, comprising the following steps: S1: crushing the raw ore with TiO2≤10.00wt% and TFe≤20.00wt%, feeding the raw ore into a powder ore dry separator for dry strong magnetic roughing to obtain the desired dry concentrate; S2: the dry concentrate is screened after high-pressure roller milling to obtain a roller product; S3: the roller product is separated by a wet magnetic separator to obtain a magnetic product and a non-magnetic product; S4: water is added to the non-magnetic product to adjust the slurry to obtain a pulp, the pulp is sent to a flotation tank, sodium hexametaphosphate is added to perform the first stirring and slurry adjustment, calcium hypochlorite is added after the first stirring and slurry adjustment is completed, and oxidation activation of the ilmenite is completed after the two stirrings; S5: a titanium concentrate composite collector M and a frother are added to the slurry that has completed the oxidation activation, and then flotation is performed, and titanium concentrate is obtained after the flotation is completed. However, this method still uses flotation technology, and it is still difficult to overcome the problems of impurities such as CaO, SiO2, Al2O3, and the problem of flotation agents being adsorbed on the mineral surface.
[0005] CN112871460A discloses a dispersion inhibitor suitable for ultrafine ilmenite, comprising hydroxyethylidene diphosphonate, sodium carboxymethyl cellulose and water glass in a mass ratio of 1:4-6:3-5. Among them, the components of the dispersion inhibitor have a certain synergistic effect, and the effect of the three combined use is significantly improved compared with the use of each component alone or separately. It is applied to the flotation separation of ultrafine ilmenite system, which can disperse the ore mud, activate ilmenite and assist in inhibiting gangue minerals (olivine, pyroxene), achieving a good flotation effect with a small dosage of reagents and a simple flotation process, thereby significantly improving the grade and recovery rate of the obtained titanium concentrate; hydroxyethylidene diphosphonate mainly bears the dispersion effect, and does not react chemically with the mineral; the sodium carboxymethyl cellulose and water glass bear the inhibitory effect of gangue minerals, and the sodium carboxymethyl cellulose also has the dispersion effect on ultrafine minerals. However, the dispersion inhibitor is not suitable for further beneficiation of ilmenite flotation concentrate.
[0006] CN117563785A discloses a flotation process for enhanced recovery of ilmenite, comprising the following steps: S1, ilmenite positive flotation: preparing ilmenite flotation raw material into ore pulp, adding positive flotation pH adjuster, ilmenite activator, ilmenite collector and frother in sequence, and carrying out "one roughing and one sweeping" positive flotation after sufficient slurrying, the obtained flotation foam product is ilmenite rough concentrate, and the product in the sweeping tank is flotation tailings 1; S2, ilmenite reverse flotation process: feeding ilmenite rough concentrate into reverse flotation process, adding reverse flotation ilmenite inhibitor and gangue collector in sequence, and carrying out "one roughing and one sweeping" reverse flotation after sufficient slurrying, the obtained product in the roughing tank is final ilmenite concentrate, and the reverse flotation foam product is tailings 2; wherein the TiO2 grade in the ilmenite flotation raw material is 16.50-21.5 0%, the gangue mineral content in the ilmenite flotation raw material is 54.00-68.00%, and the gangue minerals include titanium pyroxene, feldspar and chlorite; in S1, during roughing, the pH adjuster is sodium carbonate, and the pH value of the pulp is 7.5-8.0; the ilmenite activator is lead nitrate, and the dosage is 300-400 g / t; the ilmenite collector is a hydroxamic acid collector, and the dosage is 1500-2000 g / t; the frother is 2# oil, and the dosage is 30-40 g / t; during scavenging, the pH adjuster is sodium carbonate, and the pH value of the pulp is 7.5-8.0; the ilmenite activator is lead nitrate, and the dosage is 150-200 g / t; the ilmenite collector is a hydroxamic acid collector, and the dosage is 500-700 g / t; the frother is 2# oil, and the dosage is 10-20 g / t. However, during the entire process of this method, the environment needs to be changed from acidic to alkaline, which results in a large amount of alkali consumption, an increase in ions in the slurry, high production costs, and difficult to control water circulation. Summary of the invention
[0007] In order to overcome the problems of the prior art and achieve the goal of significantly reducing CaO, SiO2 and Al2O3 in ilmenite flotation concentrate while improving the TiO2 grade of titanium concentrate, the present invention studies and compares CaO, NaOH, Na2CO3, water glass, sodium hexametaphosphate, NaHCO3 and other reagents, and optimizes the best reagent combination suitable for flotation titanium concentrate removal, solves the flocculant problem of flotation titanium concentrate in the ore pulp, and achieves the purpose of preparing high-quality titanium concentrate using flotation titanium concentrate through screening-size classification gravity separation.
[0008] The present invention provides a method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate, which comprises the following steps:
[0009] A. The ilmenite flotation concentrate is prepared into a pulp with a mass concentration of 50% to 60%, and the ilmenite flotation concentrate is added into a stirring barrel 1 with a circulation hole and a spoiler at a flow rate of 0.75 to 1.0 kg of ilmenite flotation concentrate / min;
[0010] B. Add reagent A into stirring barrel 1 at a flow rate of 7.5 mL / min to 30 mL / min to mix reagent A and ilmenite flotation concentrate slurry evenly;
[0011] C. The slurry in the mixing barrel 1 flows by gravity into the mixing barrel 2 with circulation holes and spoilers;
[0012] D. Add reagent B into stirring barrel 2 at a flow rate of 2.25 mL / min to 5 mL / min to mix reagent B and slurry evenly;
[0013] E. The slurry in the mixing barrel 2 flows by gravity into the mixing barrel 3 with circulation holes and spoilers to further mix the slurry;
[0014] F. The slurry in the mixing barrel 3 flows into the pump by gravity, and then is pumped to the ultrasonic three-layer vibrating screen. The aperture of the upper screen is 0.15mm, the aperture of the middle screen is 0.074mm, and the aperture of the lower screen is 0.038mm, and materials with three particle sizes of +0.15mm, -0.15+0.074mm and -0.074mm+0.038mm are obtained;
[0015] G. Feed the +0.15mm and -0.15+0.074mm particle size materials into the Yunnan Tin Ore Sludge Shaking Table, respectively, and feed the -0.074mm+0.038mm particle size materials into the Yunnan Tin Fine Sludge Shaking Table for gravity separation. The shaking table gravity separation process is one-stage roughing and three-stage scavenging. The roughing concentrate is used as high-quality titanium concentrate, and the scavenging concentrate is combined with the -0.038mm particle size material as a medium-grade titanium concentrate, and the tailings are combined into total tailings;
[0016] The agent A is an aqueous solution of sodium carbonate, potassium carbonate, sodium bicarbonate or potassium bicarbonate with a mass concentration of 5% to 15%; the agent B is an aqueous solution of water glass with a modulus of 2.0 to 3.2 with a mass concentration of 5% to 15%.
[0017] Wherein, in the above method, in step A, the ilmenite flotation concentrate contains the following components in mass percentage: C 0.063%, TFe 34.23%, SiO2 2.50%, CaO 0.83%, MgO 4.93%, Al2O3 0.98%, TiO247.64%, S0.109%, Co 0.011%, Ni 0.001%, Cu 0.009%, Na2O 0.125%, K2O 0.037%, As0.003%, P <0.01%.
[0018] Wherein, in the above method, in step A, in the ilmenite flotation concentrate, ilmenite accounts for 93.75wt%, labradorite accounts for 1.50wt%, amphibole accounts for 1.42wt%, pyroxene accounts for 1.05wt%, sphene accounts for 0.86wt%, titanomagnetite accounts for 0.75wt%, olivine accounts for 0.20wt% and pyrrhotite accounts for 0.19wt%.
[0019] Wherein, in the above method, the rotation speed of the stirring barrel 1 is controlled to be 1000-1500 rad / min.
[0020] Wherein, in the above method, the rotation speed of the stirring barrel 2 is controlled to be 1000-1500 rad / min.
[0021] Wherein, in the above method, the rotation speed of the stirring barrel 3 is controlled to be 1000-1500 rad / min.
[0022] Among them, in the above method, in step G, the component contents of the obtained high-quality titanium concentrate are TiO2≥50wt%, SiO2≤1wt%, CaO≤0.15wt%, Al2O3≤0.4wt%, S≤0.05wt%, C≤0.03wt%, and the remainder is iron and unavoidable impurities.
[0023] Among them, in the above method, in step G, the component contents of the obtained medium-quality titanium concentrate are TiO2≥47wt%, SiO2≤2.5wt%, CaO≤0.8wt%, Al2O3≤1.0wt%, S≤0.20wt%, and the remainder is iron and unavoidable impurities.
[0024] Wherein, in the above method, in step G, the obtained tailings contains TiO2≤6.0wt%.
[0025] The effects achieved by the implementation of the patent of this invention are:
[0026] The present invention adopts a method of one-time dosing stirring-two-time dosing stirring-three-time stirring-ultrasonic high-frequency screening classification-shaking table to disperse the flotation titanium concentrate, thereby achieving full separation of ilmenite and gangue minerals, and obtaining high-quality titanium concentrate and medium-quality titanium concentrate, wherein the tailings contain only very little TiO2, and the tailings loss rate is 0.29%; the content of CaO, SiO2 and Al2O3 in the high-quality titanium concentrate is significantly reduced, which is beneficial to the subsequent titanium concentrate processing process, obtains high-quality titanium concentrate, and at the same time lays the foundation for further economic utilization of ilmenite flotation concentrate, and has great economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a schematic diagram of the process flow of Example 1 of the present invention. DETAILED DESCRIPTION
[0028] Specifically, a method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate comprises the following steps:
[0029] A. The ilmenite flotation concentrate is prepared into a pulp with a mass concentration of 50% to 60%, and the ilmenite flotation concentrate is added into a stirring barrel 1 with a circulation hole and a spoiler at a flow rate of 0.75 to 1.0 kg of ilmenite flotation concentrate / min;
[0030] B. Add reagent A into stirring barrel 1 at a flow rate of 7.5 mL / min to 30 mL / min to mix reagent A and ilmenite flotation concentrate slurry evenly;
[0031] C. The slurry in the mixing barrel 1 flows by gravity into the mixing barrel 2 with circulation holes and spoilers;
[0032] D. Add reagent B into stirring barrel 2 at a flow rate of 2.25 mL / min to 5 mL / min to mix reagent B and slurry evenly;
[0033] E. The slurry in the mixing barrel 2 flows by gravity into the mixing barrel 3 with circulation holes and spoilers to further mix the slurry;
[0034] F. The slurry in the mixing barrel 3 flows into the pump by gravity, and then is pumped to the ultrasonic three-layer vibrating screen. The aperture of the upper screen is 0.15mm, the aperture of the middle screen is 0.074mm, and the aperture of the lower screen is 0.038mm, and materials with three particle sizes of +0.15mm, -0.15+0.074mm and -0.074mm+0.038mm are obtained;
[0035] G. Feed the +0.15mm and -0.15+0.074mm particle size materials into the Yunnan Tin Ore Sludge Shaking Table, respectively, and feed the -0.074mm+0.038mm particle size materials into the Yunnan Tin Fine Sludge Shaking Table for gravity separation. The shaking table gravity separation process is one-stage roughing and three-stage scavenging. The roughing concentrate is used as high-quality titanium concentrate, and the scavenging concentrate is combined with the -0.038mm particle size material as a medium-grade titanium concentrate, and the tailings are combined into total tailings;
[0036] The agent A is an aqueous solution of sodium carbonate, potassium carbonate, sodium bicarbonate or potassium bicarbonate with a mass concentration of 5% to 15%; the agent B is an aqueous solution of water glass with a modulus of 2.0 to 3.2 with a mass concentration of 5% to 15%.
[0037] The main mineral in ilmenite flotation concentrate is ilmenite. The chemical molecular structure of ilmenite is FeTiO3. Theoretically, the TiO2 content is 52.66% and the FeO content is 47.34%. However, in the actual mineralization process, Mg 2+ , Ca 2+ , Mn 4+ and Mn 2+ Will be with Fe2+ The isomorphous formation of magnesia-titanium ore, perovskite and erythromanganese-titanium ore occurs. Therefore, the calcium, magnesium and manganese contents, especially the calcium and magnesium contents, in the titanium concentrate produced from the vanadium-titanium magnetite in the Panzhihua area are relatively high. At the same time, during the crushing and separation process of the ore, it is impossible for the mineral particles to be 100% dissociated. The ilmenite particles will inevitably be interbred with titano-magnetite, pyrrhotite, pyroxene, olivine, feldspar, chlorite, hornblende, magnesia-aluminum spinel, etc. into the titanium concentrate, resulting in the ilmenite flotation concentrate containing high levels of impurities such as SiO2, Al2O3, CaO, MgO, etc.
[0038] The ilmenite flotation concentrate raw material in the present invention can be prepared by conventional flotation procedures in the art through vanadium-titanium magnetite ore mined from mines. The general preparation process of ilmenite flotation concentrate is as follows: the vanadium-titanium magnetite ore (particle size 350-1000mm, TFe grade 15%-30%, TiO2 grade 5%-12%) mined from the mine is crushed to 0-12mm in a three-stage one closed circuit, three-stage grinding and three-stage weak magnetic grinding, and magnetic separation and iron selection process to obtain vanadium-titanium-iron concentrate and iron selection tailings (TFe grade 9%-13%, TiO2 grade 4%-10%). The iron selection tailings are then subjected to weak magnetic iron removal-strong magnetic pre-enrichment of ilmenite-strong magnetic titanium rough concentrate flotation desulfurization-desulfurization titanium rough concentrate flotation titanium selection to obtain ilmenite flotation concentrate slurry. The ilmenite flotation concentrate slurry is concentrated, filtered and dried to obtain ilmenite flotation concentrate (TiO2 grade is usually ≥46.5%). Based on this process, as in step A of Example 1 of the present invention, the ilmenite flotation concentrate slurry in the ilmenite flotation concentrate preparation process can actually be directly used and adjusted to the concentration required by the present invention.
[0039] In the embodiment of the present invention, the ilmenite flotation concentrate used contains the following components in percentage by mass: C 0.063%, TFe 34.23%, SiO2 2.50%, CaO 0.83%, MgO 4.93%, Al2O3 0.98%, TiO247.64%, S 0.109%, Co 0.011%, Ni 0.001%, Cu 0.009%, Na2O 0.125%, K2O 0.037%, As 0.003%, and P < 0.01%. In the ilmenite flotation concentrate, ilmenite accounts for 93.75wt%, labradorite accounts for 1.50wt%, amphibole accounts for 1.42wt%, pyroxene accounts for 1.05wt%, titanite accounts for 0.86wt%, titanomagnetite accounts for 0.75wt%, olivine accounts for 0.20wt% and pyrrhotite accounts for 0.19wt%. However, the method of the present invention is not limited to the ilmenite flotation concentrate of the embodiment.
[0040] The method of the present invention is carried out continuously, and the purpose of controlling the proportion of each material is achieved by controlling the flow rate of the ilmenite flotation concentrate slurry, reagent A, and reagent B. In step A, the flow rate of the ilmenite flotation concentrate is controlled to be 0.75-1.0 kg of ilmenite flotation concentrate / min, and in step A, the flow rate of reagent A is controlled to be 7.5 mL / min-30 mL / min, so that the amount of carbonate used is 1000-3000 g of carbonate / t of ilmenite flotation concentrate. Carbonate not only acts as a pH adjuster to dissolve the collector in the ore pulp solution in an ionic state, but more importantly, carbonate also acts as a dispersant and competitively adsorbs on the surface of ilmenite particles. CO3 in the solution 2- Fe 2+ and Ti 4+ The ions react chemically to produce water-insoluble and hydrophilic FeCO3 and Ti(CO3)2 and their complexes.
[0041] Meanwhile, in step D, the flow rate of reagent B is controlled to be 2.25 mL / min to 5 mL / min, so that the amount of water glass used is 300 to 500 g water glass / t ilmenite flotation concentrate. 2- Special dispersion properties in aqueous solution, and SiO3 2- The principle of competitive adsorption with collector ions on the surface of mineral particles.
[0042] The method of adding agent A and agent B can use a stainless steel container with a valve in the embodiment of the present invention to control its flow rate; or a stainless steel container with a stainless steel tube can be used to drip agent A, and a stainless steel container with a latex tube can be used to drip agent B.
[0043] In addition, the stirring barrels 1 to 3 used in the present invention are all equipped with circulation holes and spoilers, so that the slurry and the reagent are fully mixed to achieve the effect of removing the reagent and ensure the continuous and stable progress of the process. In addition, the rotation speed of the stirring barrel 1 is controlled to be 1000-1500 rad / min to ensure the uniform dispersion of the ilmenite flotation concentrate slurry and its uniform mixing with the reagent A; the rotation speed of the stirring barrel 2 is controlled to be 1000-1500 rad / min to ensure the uniform mixing of the slurry and the reagent B; the rotation speed of the stirring barrel 3 is controlled to be 1000-1500 rad / min to appropriately extend the processing time and further mix the slurry.
[0044] In step F of the present invention, after classification by three layers of ultrasonic vibrating screens, materials with four particle sizes of +0.15 mm, -0.15+0.074 mm, -0.074 mm+0.038 mm and -0.038 mm are obtained; among them, materials with three particle sizes of +0.15 mm, -0.15+0.074 mm and -0.074 mm+0.038 mm need to be reselected in one step. The +0.15mm and -0.15+0.074mm particle sizes are respectively fed into the Yunnan Tin Ore Sludge Shaking Table for gravity separation. The gravity separation process consists of one roughing separation and three scavenging separations. The +0.15mm roughing concentrate is used as high-quality titanium concentrate 1, and the -0.15+0.074mm roughing concentrate is used as high-quality titanium concentrate 2; the +0.15mm scavenging concentrate is used as medium-quality titanium concentrate 1, and the -0.15+0.074mm scavenging concentrate is used as medium-quality titanium concentrate 2; the +0.15mm scavenging tailings are used as tailings 1, and the -0.15+0.074mm scavenging tailings are used as tailings 2. The -0.074+0.038mm particle size is fed into the Yunxi fine mud shaker for gravity separation. The gravity separation process is one stage of roughing and three stages of scavenging. The -0.074+0.038mm particle size roughing concentrate is used as high-quality titanium concentrate 3, the -0.074+0.038mm particle size scavenging concentrate is used as medium-quality titanium concentrate 3, and the -0.074+0.038mm particle size scavenging tailings is tailings 3. The -0.038mm particle size material is used as medium-quality titanium concentrate 4. The high-quality titanium concentrates 1, 2 and 3 are combined into the total high-quality titanium concentrate, the medium-quality titanium concentrates 1, 2, 3 and the -0.038mm particle size product are combined into the total medium-quality titanium concentrate, and the scavenging tailings 1, 2 and 3 are combined into the total tailings.
[0045] In step G of the present invention, the content of the components of the obtained high-quality titanium concentrate is TiO2≥50wt%, SiO2≤1wt%, CaO≤0.15wt%, Al2O3≤0.4wt%, S≤0.05wt%, C≤0.03wt%, and the balance is iron and inevitable impurities. In step G of the present invention, the content of the components of the obtained medium-quality titanium concentrate is TiO2≥47wt%, SiO2≤2.5wt%, CaO≤0.8wt%, Al2O3≤1.0wt%, S≤0.20wt%, and the balance is iron and inevitable impurities. In step G of the present invention, the obtained tailings contain TiO2≤6.0wt%.
[0046] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the scope of the examples.
[0047] Test Example 1
[0048] Because the flotation collector is adsorbed on the surface of the ilmenite flotation concentrate particles, they agglomerate in the ore pulp and have strong hydrophobicity, making it impossible to achieve screening and classification. Therefore, this test case first conducts a test on reducing the hydrophobicity of the particle surface of the ilmenite flotation concentrate. The test process is as follows:
[0049] ① Weigh 100g of ilmenite flotation concentrate sample;
[0050] ②Put the sample into a beaker, add 200mL of deionized water to adjust the liquid-solid ratio to 2:1, add additives as required, stir evenly with a glass rod, and let stand for 10 minutes;
[0051] ③ Filter the treated slurry and rinse the filter cake with 150 mL of deionized water three times;
[0052] ④Put the filtered cake in an oven and dry it at 65℃ until it reaches constant weight;
[0053] ⑤ Weigh 5g of the treated sample and use a high-pressure tablet press to press the sample into a round cake shape to meet the requirements of the spinning drop interfacial tension tester for measuring the contact angle of the mineral surface;
[0054] ⑥ The contact angle of the pressed sample is measured using a spinning drop interfacial tension meter to determine the change pattern of the hydrophilicity (hydrophobicity) of the ilmenite surface after the action of the agent.
[0055] The results of the test on the type and amount of additives, slurry pH and contact angle of sample particles are shown in Table 1.
[0056] Table 1 Test results of types of additives for flotation of titanium concentrate
[0057] serial number Additive type and dosage Slurry pH Contact angle of mineral particle surface (°) 1 No Addition 6.0 125.00 2 CaO: 2.0g 12.5 118.00 3 <![CDATA[Na2CO3:1g;Na2SiO3:1g]]> 11.5 71.68 4 NaOH: 1g 13.0 118.00 5 <![CDATA[NaOH:1g;Na2SiO3:1g]]> 13.0 106.50 6 <![CDATA[NaHCO3:1g;Na2SiO3:1g]]> 11.0 103.54
[0058] It can be seen from Table 1 that the addition of CaO, Na2CO3+Na2SiO3, NaOH and NaOH+Na2SiO3 can reduce the surface hydrophobicity of the flotation titanium concentrate particles, among which the reduction in the surface hydrophobicity of the sample particles is most obvious when Na2CO3+Na2SiO3 is added.
[0059] Example 1
[0060] The main physical and chemical properties of the ore described in this example are:
[0061] The ilmenite flotation concentrate contains C 0.063%, TFe 34.23%, SiO2 2.50%, CaO 0.83%, MgO4.93%, Al2O30.98%, TiO2 47.64%, S 0.109%, Co 0.011%, Ni 0.001%, Cu 0.009%, Na2O 0.125%, K2O 0.037%, As 0.003%, P < 0.01%. The ilmenite flotation concentrate contains 93.75% ilmenite, 1.50% labradorite, 1.42% hornblende, 1.05% pyroxene, 0.86% sphene, 0.75% titanomagnetite, 0.20% olivine, and 0.19% pyrrhotite.
[0062] The scale of this embodiment is a laboratory-scale continuous pilot test, the raw material is the ilmenite flotation concentrate slurry produced on site, and the processing capacity is 50kg of ilmenite flotation concentrate dry ore / h. The test process is as follows:
[0063] 1) Place the prepared Na2CO3 aqueous solution with a mass concentration of 10% in a stainless steel container 1 with a capacity of 10L and a valve;
[0064] 2) Place the prepared water glass aqueous solution with a mass concentration of 10% in a stainless steel container 2 with a capacity of 10L and a valve;
[0065] 3) Place the ilmenite flotation concentrate slurry with a mass concentration of 50% to 60% in a 30L stirring barrel 1, control the slurry flow rate to 0.85L / min (about 50kg of ilmenite flotation concentrate dry ore / h), and adjust the main shaft speed of stirring 1 to 1200rad / min;
[0066] 4) Open the valve of stainless steel container 1 to allow the Na2CO3 aqueous solution to flow into the stirring barrel 1 by gravity, and adjust the flow rate of the Na2CO3 aqueous solution to 16.7 mL / min (about 2000 g Na2CO3 / t ilmenite flotation concentrate);
[0067] 5) The slurry in mixing barrel 1 flows into mixing barrel 2 by gravity, and the main shaft speed of mixing barrel 2 is adjusted to 1200rad / min;
[0068] 6) Open the valve of the stainless steel container 2 to allow the water glass aqueous solution to flow into the stirring barrel 2 by gravity, and adjust the flow rate of the water glass aqueous solution to 3.4 mL / min (about 400 g water glass / t ilmenite flotation concentrate);
[0069] 7) The slurry in mixing barrel 2 flows into mixing barrel 3 by gravity, and the main shaft speed of mixing barrel 3 is adjusted to 1200 rad / min;
[0070] 8) The slurry flows into the mixing tank 3 by gravity and is pumped to the KM-800-4s ultrasonic three-layer vibrating screen by the XBSL1 / 4 vertical sand pump. The aperture of the upper screen is 0.15mm, the aperture of the middle screen is 0.074mm, and the aperture of the lower screen is 0.038mm;
[0071] 9) The +0.15mm and -0.15+0.074mm particle sizes are fed into the 2100×1050 Yunnan Tin Ore Sludge Shaker for gravity separation. The process is one-stage roughing and three-stage scavenging. The roughing concentrate is used as high-quality titanium concentrate 1 and high-quality titanium concentrate 2, the scavenging concentrate is used as medium-quality titanium concentrate 1 and medium-quality titanium concentrate 2, and the scavenging tailings are tailings 1 and tailings 2;
[0072] 10) The -0.074+0.038mm particle size is fed into a 2100×1050 type Yunnan Tin fine mud shaking table for gravity separation. The process is one stage of roughing and three stages of scavenging. The roughing concentrate is used as high-quality titanium concentrate 3, the scavenging concentrate is used as medium-quality titanium concentrate 3, and the scavenging tailings are tailings 3;
[0073] 11) -0.038mm particle size product is used as medium quality titanium concentrate 4;
[0074] 12) Combine high-quality titanium concentrates 1, 2 and 3 into total high-quality titanium concentrates, combine medium-quality titanium concentrates 1, 2, 3 and -0.038 mm particle size products into total medium-quality titanium concentrates, and combine scavenging tailings 1, 2 and 3 into total tailings.
[0075] Example 1 process flow Figure 1 The results are shown in Table 2.
[0076] Table 2 Experimental results of Example 1
[0077]
[0078] The present invention utilizes the above process to produce two types of titanium concentrate products, high and medium, with TiO2 grades of 50.24% and 47.38%, from flotation titanium concentrate with a TiO2 grade of 47.64%, without significantly affecting the overall utilization rate of flotation titanium concentrate (the loss rate of TiO2 in tailings is 0.29%). Among them, SiO2, CaO and Al2O3 of the titanium concentrate with a TiO2 grade of 50.24% meet the requirements of boiling chlorination, and the titanium concentrate product with a TiO2 grade of 47.38% can continue to be used for molten salt chlorination.
Claims
1. A method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate, characterized in that: The following steps are involved: A. The ilmenite flotation concentrate is prepared into a pulp with a mass concentration of 50% to 60%, and the ilmenite flotation concentrate is added into a stirring barrel 1 with a circulation hole and a spoiler at a flow rate of 0.75 to 1.0 kg of ilmenite flotation concentrate / min; B. Add reagent A into stirring barrel 1 at a flow rate of 7.5 mL / min to 30 mL / min to mix reagent A and ilmenite flotation concentrate slurry evenly; C. The slurry in the mixing barrel 1 flows by gravity into the mixing barrel 2 with circulation holes and spoilers; D. Add reagent B into stirring barrel 2 at a flow rate of 2.25 mL / min to 5 mL / min to mix reagent B and slurry evenly; E. The slurry in the mixing barrel 2 flows by gravity into the mixing barrel 3 with circulation holes and spoilers to further mix the slurry; F. The slurry in the mixing barrel 3 flows into the pump by gravity, and then is pumped to the ultrasonic three-layer vibrating screen. The aperture of the upper screen is 0.15mm, the aperture of the middle screen is 0.074mm, and the aperture of the lower screen is 0.038mm, and materials with three particle sizes of +0.15mm, -0.15+0.074mm and -0.074mm+0.038mm are obtained; G. Feed the +0.15mm and -0.15+0.074mm particle size materials into the Yunnan Tin Ore Sludge Shaking Table, respectively, and feed the -0.074mm+0.038mm particle size materials into the Yunnan Tin Fine Sludge Shaking Table for gravity separation. The shaking table gravity separation process is one-stage roughing and three-stage scavenging. The roughing concentrate is used as high-quality titanium concentrate, and the scavenging concentrate is combined with the -0.038mm particle size material as a medium-grade titanium concentrate, and the tailings are combined into total tailings; The agent A is an aqueous solution of sodium carbonate, potassium carbonate, sodium bicarbonate or potassium bicarbonate with a mass concentration of 5% to 15%; the agent B is an aqueous solution of water glass with a modulus of 2.0 to 3.2 with a mass concentration of 5% to 15%.
2. The method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate according to claim 1, characterized in that: In step A, the ilmenite flotation concentrate contains the following components in percentage by mass: C 0.063%, TFe 34.23%, SiO2 2.50%, CaO 0.83%, MgO 4.93%, Al2O3 0.98%, TiO2 47.64%, S 0.109%, Co0.011%, Ni 0.001%, Cu 0.009%, Na2O 0.125%, K2O 0.037%, As 0.003%, P < 0.01%.
3. The method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate according to claim 1, characterized in that: In step A, in the ilmenite flotation concentrate, ilmenite accounts for 93.75wt%, labradorite accounts for 1.50wt%, amphibole accounts for 1.42wt%, pyroxene accounts for 1.05wt%, sphene accounts for 0.86wt%, titanomagnetite accounts for 0.75wt%, olivine accounts for 0.20wt% and pyrrhotite accounts for 0.19wt%.
4. The method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate according to claim 1, characterized in that: The rotation speed of the stirring barrel 1 is controlled to be 1000-1500 rad / min.
5. The method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate according to claim 1, characterized in that: The rotation speed of the stirring barrel 2 is controlled to be 1000-1500 rad / min.
6. The method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate according to claim 1, characterized in that: The rotation speed of the stirring barrel 3 is controlled to be 1000-1500 rad / min.
7. The method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate according to claim 1, characterized in that: In step G, the components of the obtained high-quality titanium concentrate are TiO2≥50wt%, SiO2≤1wt%, CaO≤0.15wt%, Al2O3≤0.4wt%, S≤0.05wt%, C≤0.03wt%, and the remainder is iron and unavoidable impurities.
8. The method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate according to claim 1, characterized in that: In step G, the composition content of the obtained medium-quality titanium concentrate is TiO2≥47wt%, SiO2≤2.5wt%, CaO≤0.8wt%, Al2O3≤1.0wt%, S≤0.20wt%, and the remainder is iron and unavoidable impurities.
9. The method for preparing high-quality titanium concentrate by using ilmenite flotation concentrate according to any one of claims 1 to 8, characterized in that: In step G, the obtained tailings contain TiO2≤6.0wt%.
Citation Information
Patent Citations
Ilmenite flotation method
CN105964413A
Ilmenite beneficiation method
CN109046759A
Low-grade ilmenite beneficiation process
CN117483097A
Zircon-rutile-ilmenite froth flotation process
US5106489A
Method for pre-treating ilmenite tailings after iron-beneficiation
WO2014117300A1
Cited By
Titanium middling physical and chemical coupling enhanced upgrading method
CN119702257A