Fatty acid type modified agent for fluorite flotation and preparation method and application of fatty acid type modified agent

By designing a modified agent containing fatty acids with carbon chain lengths of 12-18, monoethanolamine or diethanolamine, sodium hydroxide and OP-10, the fluorite flotation agent in the prior art is difficult to catch low-grade fireflies. The problem of stone has improved the grade and recovery rate of fluorite concentrate, and is suitable for the efficient development of complex fluorite resources.

CN118874696APending Publication Date: 2024-11-01INNER MONGOLIA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411291477.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing fluorite flotation agents are difficult to effectively capture low-grade and complex fluorite resources, and their difficulty withstand low temperatures and low water solubility limits their application, resulting in low fluorite concentrate recovery.

Method used

A fatty acid-based modification agent was designed, and it was prepared by heating, stirring and standing steps such as standing by fatty acids with carbon chain lengths of 12-18, monoethanolamine or diethanolamine, sodium hydroxide and OP-10. It can improve its selectivity and capture ability by adding non-ionic surfactants to the agent.

Benefits of technology

It has achieved high selective capture of fluorite minerals, improved the grade and recovery rate of fluorite concentrates, and is highly applicable to the efficient development of low-grade complex fluorite resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874696A_ABST
    Figure CN118874696A_ABST
Patent Text Reader

Abstract

The invention provides a fatty acid type modifying agent for fluorite flotation and a preparation method and application thereof.The fatty acid type modifying agent for fluorite flotation is prepared from fatty acid with the carbon chain length being 12-18, monoethanolamine or diethanolamine, sodium hydroxide and OP-10 according to a proper weight ratio. The preparation method comprises the following steps: adding monoethanolamine or diethanolamine into fatty acid with the carbon chain length of 12-18, heating, stirring, mixing and reacting to obtain a first mixed material, adding sodium hydroxide into the first mixed material, and heating, stirring and reacting to obtain a second mixed material; and after the second mixed material is cooled, an obtained solid is added into OP-10 and fully stirred, the finally prepared fatty acid type modifying agent for fluorite flotation is easy to dissolve in water and high in water solubility, during flotation operation, fluorite minerals are good in selectivity and high in collecting capacity, meanwhile, a nonionic surfactant is added into the agent, and the flotation efficiency is improved. The stability is good, and the applicability is high.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention belongs to the technical field of flotation reagents, and in particular relates to a fatty acid modified reagent for flotation of fluorite, and a preparation method and application thereof. Background Art

[0002] Fluorite is the only natural mineral that can be used to extract fluorine in large quantities. It is the basic raw material for fluorine chemical industry and plays an important role in cement, metallurgy, refrigeration, aviation, medicine and other fields. With the continuous development of the world economy, the deepening of resource development and the continuous expansion of the application field of fluorine, the demand and consumption of high-quality fluorite are also showing a continuous growth trend. Therefore, high-grade and easy-to-select fluorite resources are gradually exhausted, while the efficient development and utilization of low-grade, complex and difficult-to-process fluorite resources are gradually attracting people's attention. my country has large reserves of fluorite resources and obvious resource advantages, but it is mainly low-grade complex fluorite ores and polymetallic associated fluorite ores, with low comprehensive recovery rates.

[0003] The most commonly used fluorite flotation collector is fatty acid, especially oleic acid, which has strong collecting ability but weak sorting ability, and its low resistance to low temperature and low water solubility limit its application. It is difficult to obtain qualified fluorite concentrate with existing flotation reagents. Therefore, based on the in-depth study of the mechanism of action of fluorite flotation collectors, designing and modifying new reagents that meet the characteristics of fluorite flotation is an inevitable requirement for fully developing my country's large number of associated fluorite resources. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a fatty acid modified agent for flotation of fluorite and its preparation method and application. The fatty acid modified agent for flotation of fluorite of the present invention is easily soluble in water and has strong water solubility. When performing flotation operations, it has good selectivity for fluorite minerals and strong collection ability. At the same time, a non-ionic surfactant is added inside, and it has good stability and strong applicability.

[0005] The technical solution of the present invention is:

[0006] A fatty acid modified reagent for flotation of fluorite is prepared from the following raw materials:

[0007] 10-12 parts by weight of a fatty acid having a carbon chain length of 12-18;

[0008] Monoethanolamine or diethanolamine, 3-4 parts by weight;

[0009] Sodium hydroxide, 1.5-2 parts by weight;

[0010] OP-10 (nonionic surfactant), 1-2 parts by weight.

[0011] It is further preferred that the fatty acid modified agent for flotation of fluorite is prepared using the following raw materials:

[0012] 10 parts by weight of a fatty acid having a carbon chain length of 18;

[0013] Diethanolamine, 3 parts by weight;

[0014] Sodium hydroxide, 2 parts by weight;

[0015] OP-10, 1 part by weight.

[0016] The preparation method of the fatty acid modified agent for flotation of fluorite comprises the following specific operations:

[0017] (1) taking a fatty acid having a carbon chain length of 12 to 18, adding monoethanolamine or diethanolamine, heating and stirring to react, and obtaining a first mixed material;

[0018] (2) adding sodium hydroxide (preparing the sodium hydroxide of the formula mass into a sodium hydroxide solution with a concentration of 20 wt %) to the first mixed material of step (1), heating and stirring to react, and obtaining a second mixed material;

[0019] (3) cooling the second mixed material in step (2) and allowing it to stand, separating the solid from the liquid, and then taking out the solid for later use;

[0020] (4) Add OP-10 to the solid obtained in step (3), and stir the mixture thoroughly to obtain the fatty acid modified agent for flotation of fluorite.

[0021] In step (1), the heating temperature is 70-80° C. and the stirring time is 1-2 h.

[0022] In step (2), the heating temperature is 70-80° C. and the stirring time is 20-30 min.

[0023] In step (3), the standing time is 10-30 min.

[0024] The application of the fatty acid modification agent in fluorite flotation.

[0025] The beneficial effects of the present invention are:

[0026] The invention provides a fatty acid modified agent for flotation of fluorite. The raw material components include fatty acid with a carbon chain length of 12-18, monoethanolamine or diethanolamine, sodium hydroxide and OP-10 in an appropriate weight ratio. During preparation, monoethanolamine or diethanolamine is first added to the fatty acid with a carbon chain length of 12-18 to carry out heating, stirring and mixing reaction to obtain a first mixed material. Then, sodium hydroxide is added to the first mixed material to carry out heating, stirring and reaction to obtain a second mixed material. The solid obtained after cooling the second mixed material is added with OP-10 and fully stirred. The finally prepared fatty acid modified agent for flotation of fluorite is easily soluble in water and has strong water solubility. When performing flotation operation, the agent has good selectivity for fluorite minerals and strong collection ability. At the same time, a non-ionic surfactant is added inside the agent, and the agent has good stability and strong applicability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 Shown is a flotation flow chart of the fatty acid modified reagent described in the present invention for flotation of fluorite. DETAILED DESCRIPTION

[0029] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0030] The above technical solution is described in detail below in conjunction with specific embodiments.

[0031] In the following examples, 1 part by weight represents 1 g.

[0032] Example 1

[0033] This embodiment provides a fatty acid modified reagent for flotation of fluorite, and its raw material composition is as follows:

[0034] 10 parts by weight of a fatty acid having a carbon chain length of 18;

[0035] Monoethanolamine, 3 parts by weight;

[0036] Sodium hydroxide, 2 parts by weight;

[0037] OP-10, 1 part by weight.

[0038] Furthermore, the method for preparing the fatty acid modified agent for flotation of fluorite comprises the following steps:

[0039] (1) placing the above-mentioned weight of fatty acid with a carbon chain length of 18 in a reaction kettle, and then adding the above-mentioned weight of monoethanolamine in the reaction kettle, heating and stirring the mixture, the heating temperature is 80° C., and stirring for 2 hours to fully blend the two, thereby obtaining a first mixed material;

[0040] (2) preparing a sodium hydroxide solution with a concentration of 20 wt % by weight of the sodium hydroxide, adding the prepared sodium hydroxide solution to the first mixed material, heating and stirring the mixed material at a temperature of 80° C. for 30 min to fully mix the mixed material, and obtaining a second mixed material;

[0041] (3) cooling the second mixed material and allowing it to stand for 30 minutes, separating the solid from the liquid, and then taking out the solid for later use;

[0042] (4) Add the above-mentioned weight of OP-10 to the solid obtained in step (3), and stir it evenly to obtain the fatty acid modified agent for flotation of fluorite.

[0043] In the above preparation method, the temperature and pressure in the reaction kettle are both low temperature and normal pressure.

[0044] The modified reagent was applied in industrial tests. The actual fluorite content in the raw mineral ore is 21.14%. In addition, other main minerals are magnetite (hematite), rare earth minerals, carbonate minerals, silicate minerals, etc. The flotation flow chart is as follows Figure 1 The specific addition amount of each agent in each treatment process is shown in Table 1.

[0045] Through the one-coarse-four-fine open-circuit test in Example 1, a fluorite concentrate with a CaF2 grade of 82.45% and an operating recovery rate of 13.06% was obtained.

[0046] Example 2

[0047] This embodiment provides a fatty acid modified reagent for flotation of fluorite, and its raw material composition is as follows:

[0048] Palmitic acid with a carbon chain length of 16, 12 parts by weight;

[0049] Monoethanolamine, 3 parts by weight;

[0050] Sodium hydroxide, 2 parts by weight;

[0051] OP-10, 1 part by weight.

[0052] Furthermore, the method for preparing the fatty acid modified agent for flotation of fluorite comprises the following steps:

[0053] (1) placing the above-mentioned weight of palmitic acid with a carbon chain length of 16 in a reaction kettle, and then adding the above-mentioned weight of monoethanolamine in the reaction kettle, heating and stirring the mixture, the heating temperature being 70° C., and stirring for 1.5 hours to fully blend the two, thereby obtaining a first mixed material;

[0054] (2) preparing a sodium hydroxide solution with a concentration of 20 wt % by weight of the sodium hydroxide, adding the prepared sodium hydroxide solution to the first mixed material, heating and stirring the mixed material at a temperature of 80° C. for 30 min to fully mix the mixed material, and obtaining a second mixed material;

[0055] (3) cooling the second mixed material and allowing it to stand for 30 minutes, separating the solid from the liquid, and then taking out the solid for later use;

[0056] (4) Add the above-mentioned weight of OP-10 to the solid obtained in step (3), and stir it evenly to obtain the fatty acid modified agent for flotation of fluorite.

[0057] In the above preparation method, the temperature and pressure in the reaction kettle are both low temperature and normal pressure.

[0058] Modified reagents are used in industrial tests. The actual fluorite content in the raw ore is 21.14%. In addition, other main minerals are magnetite (hematite), rare earth minerals, carbonate minerals, silicate minerals, etc. The flotation flow chart is as follows Figure 1 The specific addition amount of each agent in each treatment process is shown in Table 1.

[0059] Through the one-coarse-four-fine open-circuit test in Example 2, a fluorite concentrate with a CaF2 grade of 84.29% and an operating recovery rate of 51.53% was obtained.

[0060] Example 3

[0061] This embodiment provides a fatty acid modified reagent for flotation of fluorite, and its raw material composition is as follows:

[0062] Lauric acid with a carbon chain length of 12, 12 parts by weight;

[0063] Monoethanolamine, 4 parts by weight;

[0064] Sodium hydroxide, 2 parts by weight;

[0065] OP-10, 1 part by weight.

[0066] Furthermore, the method for preparing the fatty acid modified agent for flotation of fluorite comprises the following steps:

[0067] (1) placing the above-mentioned weight of lauric acid having a carbon chain length of 12 in a reaction kettle, and then adding the above-mentioned weight of monoethanolamine therein, heating and stirring the mixture, the heating temperature being 70° C., and stirring for 1.5 hours to fully blend the two, thereby obtaining a first mixed material;

[0068] (2) preparing a sodium hydroxide solution with a concentration of 20 wt % by weight of the sodium hydroxide, adding the prepared sodium hydroxide solution to the first mixed material, heating and stirring the mixed material at a temperature of 80° C. for 30 min to fully mix the mixed material, and obtaining a second mixed material;

[0069] (3) cooling the second mixed material and allowing it to stand for 30 minutes, separating the solid from the liquid, and then taking out the solid for later use;

[0070] (4) Add the above-mentioned weight of OP-10 to the solid obtained in step (3), and stir it evenly to obtain the fatty acid modified agent for flotation of fluorite.

[0071] In the above preparation method, the temperature and pressure in the reaction kettle are both low temperature and normal pressure.

[0072] Modified reagents are used in industrial tests. The actual fluorite content in the raw ore is 21.14%. In addition, other main minerals are magnetite (hematite), rare earth minerals, carbonate minerals, silicate minerals, etc. The flotation flow chart is as follows Figure 1 The specific addition amount of each agent in each treatment process is shown in Table 1.

[0073] Through the one-coarse-four-fine open-circuit test in Example 3, a fluorite concentrate with a CaF2 grade of 88.65% and an operating recovery rate of 37.53% was obtained.

[0074] Example 4

[0075] This embodiment provides a fatty acid modified reagent for flotation of fluorite, and its raw material composition is as follows:

[0076] Oleic acid with a carbon chain length of 18, 11 parts by weight;

[0077] Diethanolamine, 3 parts by weight;

[0078] Sodium hydroxide, 1.5 parts by weight;

[0079] OP-10, 1 part by weight.

[0080] Furthermore, the method for preparing the fatty acid modified agent for flotation of fluorite comprises the following steps:

[0081] (1) placing the above-mentioned weight of oleic acid with a carbon chain length of 18 in a reaction kettle, and then adding the above-mentioned weight of diethanolamine in the reaction kettle, heating and stirring the mixture at a temperature of 80° C. and stirring for 2 hours to fully blend the two to obtain a first mixed material;

[0082] (2) preparing a sodium hydroxide solution with a concentration of 20 wt % by weight of the sodium hydroxide, adding the prepared sodium hydroxide solution to the first mixed material, heating and stirring the mixed material at a temperature of 80° C. for 30 min to fully mix the mixed material, and obtaining a second mixed material;

[0083] (3) cooling the second mixed material and allowing it to stand for 30 minutes, separating the solid from the liquid, and then taking out the solid for later use;

[0084] (4) Add the above-mentioned weight of OP-10 to the solid obtained in step (3), and stir it evenly to obtain the fatty acid modified agent for flotation of fluorite.

[0085] In the above preparation method, the temperature and pressure in the reaction kettle are both low temperature and normal pressure.

[0086] Modified reagents are used in industrial tests. The actual fluorite content in the raw ore is 21.14%. In addition, other main minerals are magnetite (hematite), rare earth minerals, carbonate minerals, silicate minerals, etc. The flotation flow chart is as follows Figure 1 The specific addition amount of each agent in each treatment process is shown in Table 2.

[0087] Through the one-coarse-four-fine open-circuit test in Example 4, a fluorite concentrate with a CaF2 grade of 68.73% and an operating recovery rate of 75.45% was obtained.

[0088] Example 5

[0089] This embodiment provides a fatty acid modified reagent for flotation of fluorite, and its raw material composition is as follows:

[0090] Palmitic acid with a carbon chain length of 16, 10 parts by weight;

[0091] Diethanolamine, 3 parts by weight;

[0092] Sodium hydroxide, 2 parts by weight;

[0093] OP-10, 1.5 parts by weight.

[0094] Furthermore, the method for preparing the fatty acid modified agent for flotation of fluorite comprises the following steps:

[0095] (1) placing the above-mentioned weight of palmitic acid with a carbon chain length of 16 in a reaction kettle, and then adding the above-mentioned weight of diethanolamine in the reaction kettle, heating and stirring the mixture, the heating temperature being 70° C., and stirring for 1.5 hours to fully blend the two, thereby obtaining a first mixed material;

[0096] (2) preparing a sodium hydroxide solution with a concentration of 20 wt % by weight of the sodium hydroxide, adding the prepared sodium hydroxide solution to the first mixed material, heating and stirring the mixed material at a temperature of 80° C. for 30 min to fully mix the mixed material, and obtaining a second mixed material;

[0097] (3) cooling the second mixed material and allowing it to stand for 30 minutes, separating the solid from the liquid, and then taking out the solid for later use;

[0098] (4) Add the above-mentioned weight of OP-10 to the solid obtained in step (3), and stir it evenly to obtain the fatty acid modified agent for flotation of fluorite.

[0099] In the above preparation method, the temperature and pressure in the reaction kettle are both low temperature and normal pressure.

[0100] Modified reagents are used in industrial tests. The actual fluorite content in the raw ore is 21.14%. In addition, other main minerals are magnetite (hematite), rare earth minerals, carbonate minerals, silicate minerals, etc. The flotation flow chart is as follows Figure 1 The specific addition amount of each agent in each treatment process is shown in Table 2.

[0101] The one-coarse-four-fine open-circuit test in Example 5 yielded a fluorite concentrate with a CaF2 grade of 79.36% and an operating recovery rate of 47.65%.

[0102] Example 6

[0103] This embodiment provides a fatty acid modified reagent for flotation of fluorite, and its raw material composition is as follows:

[0104] Lauric acid with a carbon chain length of 12, 10 parts by weight;

[0105] Monoethanolamine, 3 parts by weight;

[0106] Sodium hydroxide, 2 parts by weight;

[0107] OP-10, 2 parts by weight.

[0108] Furthermore, the method for preparing the fatty acid modified agent for flotation of fluorite comprises the following steps:

[0109] (1) placing the above-mentioned weight of lauric acid having a carbon chain length of 12 in a reaction kettle, and then adding the above-mentioned weight of diethanolamine in the reaction kettle, heating and stirring the mixture, the heating temperature being 70° C., and stirring for 1.5 hours to fully blend the two, thereby obtaining a first mixed material;

[0110] (2) preparing a sodium hydroxide solution with a concentration of 20 wt % by weight of the sodium hydroxide, adding the prepared sodium hydroxide solution to the first mixed material, heating and stirring the mixed material at a temperature of 80° C. for 30 min to fully mix the mixed material, and obtaining a second mixed material;

[0111] (3) cooling the second mixed material and allowing it to stand for 30 minutes, separating the solid from the liquid, and then taking out the solid for later use;

[0112] (4) Add the above-mentioned weight of OP-10 to the solid obtained in step (3), and stir it evenly to obtain the fatty acid modified agent for flotation of fluorite.

[0113] In the above preparation method, the temperature and pressure in the reaction kettle are both low temperature and normal pressure.

[0114] Modified reagents are used in industrial tests. The actual fluorite content in the raw ore is 21.14%. In addition, other main minerals are magnetite (hematite), rare earth minerals, carbonate minerals, silicate minerals, etc. The flotation flow chart is as follows Figure 1 The specific addition amount of each agent in each treatment process is shown in Table 2.

[0115] The one-coarse-four-fine open-circuit test in Example 6 yielded a fluorite concentrate with a CaF2 grade of 82.52% and an operating recovery rate of 42.94%.

[0116] Table 1-Specific dosage of reagents in each treatment process in Example 1-3 one coarse four fine open circuit test

[0117]

[0118]

[0119] Table 2-Specific dosage of reagents in each treatment process in Example 4-6 one coarse four fine open circuit test

[0120]

[0121]

[0122] Comparative Example 1

[0123] This embodiment provides a fatty acid reagent for flotation of fluorite, and its raw material composition is as follows:

[0124] Palmitic acid with a carbon chain length of 16, 12 parts by weight;

[0125] Sodium hydroxide, 2 parts by weight.

[0126] Furthermore, the method for preparing sodium palmitate for flotation of fluorite comprises the following steps:

[0127] (1) placing the above-mentioned weight of palmitic acid having a carbon chain length of 16 in a reaction kettle, then adding the above-mentioned weight of sodium hydroxide in the reaction kettle, heating and stirring the reaction kettle at a heating temperature of 80° C. and stirring for 30 minutes to fully mix the reaction kettle to obtain a mixed material;

[0128] In the above preparation method, the temperature and pressure in the reaction kettle are both low temperature and normal pressure.

[0129] Sodium palmitate is used in industrial experiments. The actual fluorite content in the raw mineral is 21.14%. In addition, other main minerals are magnetite (hematite), rare earth minerals, carbonate minerals, silicate minerals, etc. The flotation flow chart is as follows Figure 1 The specific addition amount of each agent in each treatment process is shown in Table 3.

[0130] Through the one-coarse-four-fine open-circuit test of Comparative Example 1, a fluorite concentrate with a CaF2 grade of 80.02% and an operating recovery rate of 35.71% was obtained.

[0131] Comparative Example 2

[0132] This embodiment provides a fatty acid reagent for flotation of fluorite, and its raw material composition is as follows:

[0133] Lauric acid with a carbon chain length of 12, 12 parts by weight;

[0134] Sodium hydroxide, 2 parts by weight.

[0135] Furthermore, the method for preparing sodium laurate for flotation of fluorite comprises the following steps:

[0136] (1) placing the above-mentioned weight of lauric acid having a carbon chain length of 12 in a reaction kettle, then adding the above-mentioned weight of sodium hydroxide in the reaction kettle, heating and stirring the reaction kettle at a heating temperature of 80° C. and stirring for 30 minutes to fully mix the reaction kettle, thereby obtaining a second mixed material;

[0137] In the above preparation method, the temperature and pressure in the reaction kettle are both low temperature and normal pressure.

[0138] Sodium laurate is used in industrial experiments. The actual fluorite content in the raw mineral is 21.14%. In addition, other main minerals are magnetite (hematite), rare earth minerals, carbonate minerals, silicate minerals, etc. The flotation flow chart is as follows Figure 1The specific addition amount of each agent in each treatment process is shown in Table 3.

[0139] Through the one-coarse-four-fine open-circuit test of Comparative Example 2, a fluorite concentrate with a CaF2 grade of 73.48% and an operating recovery rate of 30.19% was obtained.

[0140] Comparative Example 3

[0141] This embodiment provides a fatty acid reagent for flotation of fluorite, and its raw material composition is as follows:

[0142] Oleic acid with a carbon chain length of 18, 11 parts by weight;

[0143] Sodium hydroxide, 1.5 parts by weight.

[0144] Furthermore, the method for preparing sodium oleate for flotation of fluorite comprises the following steps:

[0145] (1) placing the above-mentioned weight of oleic acid having a carbon chain length of 18 in a reaction kettle, then adding the above-mentioned weight of sodium hydroxide in the reaction kettle, heating and stirring the reaction kettle at a temperature of 80° C. and stirring for 30 minutes to fully mix the reaction kettle, thereby obtaining a second mixed material;

[0146] In the above preparation method, the temperature and pressure in the reaction kettle are both low temperature and normal pressure.

[0147] Sodium oleate is used in industrial experiments. The actual fluorite content in the raw mineral ore is 21.14%. In addition, other main minerals are magnetite (hematite), rare earth minerals, carbonate minerals, silicate minerals, etc. The flotation flow chart is as follows Figure 1 The specific addition amount of each agent in each treatment process is shown in Table 3.

[0148] Through the one-coarse-four-fine open-circuit test of Comparative Example 3, a fluorite concentrate with a CaF2 grade of 63.68% and an operating recovery rate of 60.31% was obtained.

[0149] Table 3-Specific dosage of reagents in each treatment process in comparative example 1-3 one coarse four fine open circuit test

[0150]

[0151] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A fatty acid modified agent for flotation of fluorite, characterized in that: Made from the following raw materials: 10-12 parts by weight of a fatty acid having a carbon chain length of 12-18; Monoethanolamine or diethanolamine, 3-4 parts by weight; Sodium hydroxide, 1.5-2 parts by weight; OP-10, 1-2 parts by weight.

2. The fatty acid modifying agent for flotation of fluorite according to claim 1, characterized in that: Made from the following raw materials: 10 parts by weight of a fatty acid having a carbon chain length of 18; Diethanolamine, 3 parts by weight; Sodium hydroxide, 2 parts by weight; OP-10, 1 part by weight.

3. A method for preparing a fatty acid modified agent for flotation of fluorite according to claim 1 or 2, characterized in that: The specific operations are: (1) taking a fatty acid having a carbon chain length of 12 to 18, adding monoethanolamine or diethanolamine, heating and stirring to react, and obtaining a first mixed material; (2) adding sodium hydroxide to the first mixed material in step (1), heating and stirring to react, to obtain a second mixed material; (3) cooling the second mixed material in step (2) and allowing it to stand, separating the solid from the liquid, and then taking out the solid for later use; (4) OP-10 is added to the solid obtained in step (3), and the mixture is stirred thoroughly to obtain the fatty acid modified agent for flotation of fluorite.

4. The method for preparing a fatty acid modified agent for flotation of fluorite according to claim 3, characterized in that: In step (1), the heating temperature is 70-80° C. and the stirring time is 1-2 h.

5. The method for preparing a fatty acid modified agent for flotation of fluorite according to claim 3, characterized in that: In step (2), the heating temperature is 70-80° C. and the stirring time is 20-30 min.

6. The method for preparing a fatty acid modified agent for flotation of fluorite according to claim 3, characterized in that: In step (3), the standing time is 10-30 min.

7. Use of the fatty acid modifying agent according to any one of claims 1-2 in fluorite flotation.