Treatment process and system for waste incineration slag

By weathering the waste incinerator slag and doping the iron tetraoxide reaction, a foam-like porous structure is formed and light blocks are made with cement, which solves the weight and adhesion problems of the waste incinerator slag in the building, and achieves the Lighter and stronger block effect.

CN118875002APending Publication Date: 2024-11-01SHENZHEN XIJIANG ENVIRONMENTAL PROTECTION RESOURCES DEV & UTILIZATION CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410940725.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, how to manufacture lightweight blocks through waste incineration slag is an urgent problem. When the existing waste incineration slag is used as a building material, the pore structure affects the engineering characteristics and has a large weight, which increases the construction strength.

Method used

By obtaining fresh waste incinerator slag, it is weathered and reacted with iron salts, zinc salts and other compounds to form doped iron tetraoxide, forming a foam-like porous structure, combining cement and block auxiliary materials, and forming a mechanism of autoclave and brick pressing to form a foam-like porous structure. Lightweight blocks to enhance adhesion.

Benefits of technology

The weight of the generated lightweight blocks is reduced by 5-10%, and the adhesion is enhanced, which reduces construction costs and increases the compressive strength of the blocks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875002A_ABST
    Figure CN118875002A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of waste recycling, and discloses a waste incineration slag treatment process and system. The waste incineration slag treatment process specifically comprises the following steps that S101, fresh quenched waste incineration slag is obtained and put into a closed container, the closed container is heated to 100-120 DEG C, forced ventilation is conducted for weathering treatment after heating is conducted for a period of time, cyclic heating and ventilation are conducted for 5-10 times, and air-dried incineration slag is obtained for standby application; s102, weighing ferric salt, zinc salt and ammonia monohydrate in parts by weight, grinding and smashing the ferric salt and the zinc salt, dissolving the ferric salt and the zinc salt into deionized water, mechanically stirring for 5-10 minutes, and then titrating the ammonia monohydrate into the mixed solution in sequence. Holes of the foamed porous structure formed by the invention are irregularly distributed, so that the incineration slag and a complex have an adsorption effect, the cohesive force of the incineration slag and the complex is enhanced, and meanwhile, new pores are formed through degradation of residual organic matters in the slags subjected to weathering treatment, so that the formed lightweight building block is lighter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of waste recycling, and in particular to a waste incineration slag treatment process and system thereof. Background Art

[0002] With the increase of urban land cost, the landfill method is increasingly restricted, and more and more urban domestic waste is treated by incineration. Waste incineration produces a large amount of domestic waste incineration slag. According to statistics, every ton of domestic waste incineration will produce 0.2 tons of domestic waste incineration slag. At present, a large amount of domestic waste incineration slag is used as building materials, such as civil engineering structural layer materials, cement production, bricklaying, etc.

[0003] However, the slag from the incineration of domestic waste contains a large amount of pore structure, which affects the engineering properties of the slag from the incineration of domestic waste as a building material. Concrete blocks are made of a mixture of cement and sand and gravel, which are heavy and increase the construction intensity. Therefore, lightweight blocks have come into being. They generally refer to foam bricks. Normal indoor partitions are made of this kind of bricks, which effectively reduce the load on the floor and have good sound insulation effect. Strength products are made of high-quality plate-shaped corundum and mullite as aggregates, with sillimanite composite as the matrix, and special additives and a small amount of rare earth oxides are added for mixing, and then formed under high pressure and fired at high temperature.

[0004] In the prior art, how to manufacture lightweight blocks using waste incineration slag is a technical problem that needs to be solved urgently by the present technical solution. Summary of the invention

[0005] The purpose of the present invention is to provide a waste incineration slag treatment process and system thereof. The pores of the foam-like porous structure are irregularly distributed, so that the incineration slag and the complex body are adsorbed, thereby enhancing their bonding force. The purpose is to solve the problem of how to manufacture lightweight blocks using waste incineration slag in the prior art.

[0006] The present invention is achieved by a waste incineration slag treatment process, which specifically comprises the following steps:

[0007] S101: freshly quenched waste incineration slag is obtained in a sealed container, and the sealed container is heated to 100-120° C. After heating for a period of time, forced ventilation is performed for weathering treatment, and the heating and ventilation cycle is repeated 5-10 times to obtain air-dried incineration slag for use;

[0008] S102: Weighing iron salt, zinc salt and ammonia monohydrate by weight, grinding the iron salt and zinc salt, dissolving them in deionized water, and mechanically stirring for 5-10 minutes, and then titrating ammonia monohydrate into the mixed solution in sequence, adjusting the pH of the mixed solution to 9-11, and obtaining a mixed solution;

[0009] S103: placing the mixed solution into an autoclave, adjusting the temperature of the autoclave to 230-250° C. for reaction for 5-10 hours, and adjusting the temperature of the autoclave to 130-150° C. after the reaction is completed, tempering the product for 1-2 hours, and then cooling and drying to obtain an intermediate product of ferroferric oxide;

[0010] S104: adding the ferroferric oxide intermediate product to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, mixing well, and then adding ammonium sulfate to obtain a building block auxiliary material;

[0011] S105: placing the air-dried incineration slag in a mixing box, adding auxiliary building block materials and cement into the mixing box, stirring for 3-5 hours to make the mixture evenly mixed, and then introducing it into a brick press for pressing and molding. After pressing and molding and drying, lightweight building blocks are obtained.

[0012] Further, in S101, freshly quenched waste incineration slag is obtained in a closed container, including:

[0013] Obtain the garbage to be incinerated and place it in an incinerator for preliminary draining, and then incinerate it once after the preliminary draining is completed;

[0014] After the first incineration is completed, the waste incineration slag is initially stirred, and then ignited again for secondary incineration;

[0015] Obtain the incineration slag after secondary incineration.

[0016] Furthermore, obtaining the incineration slag after secondary incineration includes:

[0017] Pour the incineration slag after secondary incineration into a ball mill for grinding;

[0018] Obtaining processed incineration slag, and placing the processed incineration slag on a vibrating screen for screening;

[0019] The particle size of the vibrating screen holes is controlled at 5-10 mm to obtain the sieved incineration slag.

[0020] Furthermore, in S102, when the iron salt and the zinc salt are mixed with deionized water, the stirring speed of the stirrer is 1800-2200 r / min, and the particle size of the iron salt and the zinc salt after being ground and crushed is 5-10 mm.

[0021] Further, in S104, the ferroferric oxide intermediate product is added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, and ammonium sulfate is added after mixing evenly, comprising:

[0022] The ferroferric oxide intermediate product is added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid and mechanically stirred for 10-15 minutes;

[0023] Continuously add ammonium sulfate to the mixed solution while stirring until the titration is complete and then stir for 10-15 minutes to obtain the building block auxiliary material.

[0024] Furthermore, in S105, the internal temperature of the brick press when pressing bricks is 110-130°C.

[0025] Mechanism of action:

[0026] Since ferroferric oxide has unique electrical and magnetic properties, when zinc is added, the particle size of the zinc-doped ferroferric oxide obtained is reduced, the dispersion is increased, the specific surface area is increased, the saturation magnetization intensity of ferroferric oxide is increased, the coercive force is reduced, and the magnetic loss capacity of ferroferric oxide is improved. During polymerization, aniline monomers will firstly polymerize on the surface of zinc-doped ferroferric oxide particles. Since the prepared zinc-doped ferroferric oxide has good dispersion, the polymers formed at the beginning are separated from each other. As the polymerization reaction proceeds, the mutual entanglement of polyaniline molecular chains makes it impossible for the formed conductive polyaniline to be completely separated from each other, thus finally forming a foam-like porous structure and a complex body with irregular pore distribution. The complex body is then combined with incineration slag and cement, so that the incineration slag and the complex body are adsorbed, thereby enhancing the bonding force. At the same time, the degradation of residual organic matter in the weathered slag will also form new pores, so that the formed lightweight building blocks are lighter.

[0027] Compared with the prior art, the waste incineration slag treatment process and system provided by the present invention have the following beneficial effects:

[0028] 1. Through the reaction of iron salt and zinc salt, zinc-doped ferroferric oxide is generated. Due to the dual effects of static electricity and hydrogen bonds, the bonding force between ferroferric oxide and aniline is enhanced, and finally a foam-like porous structure is formed with a lighter weight, thereby reducing the weight of the prepared concrete blocks. Compared with ordinary concrete blocks, the weight is reduced by 5-10%, and the pores of the foam-like porous structure are irregularly distributed, resulting in the adsorption of the incineration slag and the complex body, thereby enhancing its bonding force. At the same time, the degradation of residual organic matter in the weathered slag will also form new pores, making the formed lightweight blocks lighter;

[0029] 2. The foamy porous structure complex is easy to mix with cement. The cement adheres to the surface of the incineration slag, making the incineration slag and the block auxiliary materials bond more closely, so as to improve the strength of the generated lightweight blocks and greatly reduce the production cost of construction.

[0030] A waste incineration slag treatment system, which performs the above waste incineration slag treatment process, comprises:

[0031] The monitoring module is used to monitor the execution equipment of the waste incineration slag treatment process throughout the process to ensure that each treatment process meets the requirements;

[0032] The MCU module is used to issue and terminate instructions to the execution equipment of the waste incineration slag treatment process to implement each process link. The MCU module controls the corresponding execution equipment to complete the corresponding action output, and after the action is completed, it issues a termination signal to the execution equipment to enter the standby mode.

[0033] Specifically, the execution device includes:

[0034] Incinerators for obtaining freshly quenched waste incinerator slag;

[0035] A closed container is used to heat and weather the freshly quenched waste incineration slag to remove excess water from the waste incineration slag;

[0036] An autoclave is used to heat the mixed solution under high pressure to obtain the intermediate product of ferroferric oxide;

[0037] Mixing box, used to mix the air-dried incineration slag with auxiliary block materials and cement to form lightweight block pre-processing materials;

[0038] The brick press is used to press and shape the pre-processed materials of the lightweight building blocks, and the lightweight building blocks are obtained after pressing, molding and drying.

[0039] Specifically, the incinerator includes an incinerator and a stirring mechanism. The incinerator is used to incinerate the material in the incinerator. The monitoring module stops the incineration operation when it detects that the combustion in the incinerator is completed, and sends a signal to the stirring mechanism. The stirring mechanism stirs the material after the first incineration is completed, and then feeds back a signal to the incinerator after the stirring is completed. The incinerator performs a second incineration on the material in the incinerator again.

[0040] Specifically, the monitoring module includes:

[0041] A first monitoring unit, which is used to monitor the incineration state of the garbage in the incinerator, and obtain the progress of the garbage incineration by monitoring the smoke concentration generated during incineration and the internal temperature;

[0042] A second monitoring unit, the second monitoring unit is used to determine whether the temperature in the sealed container reaches a preset temperature;

[0043] A third monitoring unit, the third monitoring unit is used to monitor whether the reaction temperature in the autoclave reaches a preset temperature;

[0044] A fourth monitoring unit, the fourth monitoring unit is used to monitor the boring mixing time in the mixing box, and send a signal to the MCU module after the mixing time is reached, and the MCU module then sends a mixing termination signal to the mixing box;

[0045] A fifth monitoring unit, the fifth monitoring unit is used to monitor whether the internal temperature of the brick press reaches a preset temperature when pressing bricks;

[0046] The alarm unit is used to confirm the data monitored by the first monitoring unit, the second monitoring unit, the third monitoring unit, and the fifth monitoring unit, and execute an alarm function if the preset conditions are not met. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 A schematic flow chart of a waste incineration slag treatment process proposed by the present invention;

[0048] Figure 2 A schematic block diagram of the process of obtaining freshly quenched waste incineration slag in a waste incineration slag treatment process proposed by the present invention;

[0049] Figure 3 This is a schematic structural diagram of a waste incineration slag treatment system proposed by the present invention;

[0050] Figure 4 A schematic diagram of system connections of an incinerator in a waste incineration slag treatment system proposed by the present invention;

[0051] Figure 5 This is a schematic diagram of the structure of a monitoring module in a waste incineration slag processing system proposed by the present invention. DETAILED DESCRIPTION

[0052] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0053] The implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0054] The same or similar numbers in the drawings of this embodiment correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "upper", "lower", "left", "right" and the like indicate directions or positional relationships based on the directions or positional relationships shown in the drawings, it is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, the terms describing the positional relationship in the drawings are only used for illustrative purposes and cannot be understood as limitations on the present invention. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.

[0055] Example 1

[0056] Reference Figure 1-2 As shown, a waste incineration slag treatment process specifically includes the following steps:

[0057] S101: Obtain the garbage to be incinerated and place it in an incinerator for preliminary draining. After the preliminary draining is completed, perform a primary incineration; after the primary incineration is completed, perform a preliminary stirring on the garbage incineration slag, and after stirring, ignite it again for a secondary incineration; obtain the incineration slag after the secondary incineration.

[0058] Obtain incineration slag after secondary incineration, including:

[0059] Pour the incineration slag after secondary incineration into a ball mill for grinding;

[0060] Obtaining processed incineration slag, and placing the processed incineration slag on a vibrating screen for screening;

[0061] The particle size of the vibrating screen holes is controlled at 5 mm to obtain the sieved incineration slag;

[0062] The freshly quenched waste incineration slag is obtained in a sealed container, and the sealed container is heated to 100°C. After heating for a period of time, forced ventilation is performed for weathering treatment, and the heating and ventilation cycle is repeated 5 times to obtain the air-dried incineration slag for use;

[0063] S102: Weighing iron salt, zinc salt and ammonia monohydrate by weight, grinding the iron salt and zinc salt, dissolving them in deionized water, and mechanically stirring for 5 minutes, and then titrating ammonia monohydrate into the mixed solution in sequence, adjusting the pH of the mixed solution to 9, and obtaining a mixed solution;

[0064] S103: placing the mixed solution into an autoclave, adjusting the temperature of the autoclave to 230° C. for reaction for 5 hours, and adjusting the temperature of the autoclave to 130° C. after the reaction is completed, tempering the product for 1 hour, and then cooling and drying to obtain an intermediate product of ferroferric oxide;

[0065] S104: adding the ferroferric oxide intermediate product to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, mixing well, and then adding ammonium sulfate to obtain a building block auxiliary material;

[0066] S105: placing the air-dried incineration slag in a mixing box, adding auxiliary building block materials and cement into the mixing box, stirring for 3 hours to make the mixture evenly mixed, and then introducing it into a brick press for pressing and molding. After pressing and molding and drying, lightweight building blocks are obtained.

[0067] In this embodiment, when the iron salt and the zinc salt are mixed with deionized water, the stirring speed of the stirrer is 1800 r / min, and the particle size of the iron salt and the zinc salt after being ground and crushed is 5 mm.

[0068] In this embodiment, the ferroferric oxide intermediate product is added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, mixed evenly and then ammonium sulfate is added, comprising:

[0069] The ferroferric oxide intermediate product was added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid and mechanically stirred for 10 minutes;

[0070] Continuously add ammonium sulfate to the mixed solution while stirring until the titration is completed and then stir for 10 minutes to obtain the building block auxiliary material.

[0071] In this embodiment, the internal temperature of the brick press when pressing bricks is 110°C.

[0072] Example 2

[0073] Reference Figure 1-2 As shown, a waste incineration slag treatment process specifically includes the following steps:

[0074] S1 01: Obtain the garbage to be incinerated and place it in an incinerator, perform preliminary draining, and perform a primary incineration after the preliminary draining is completed; after the primary incineration is completed, perform preliminary stirring on the garbage incineration slag, and after stirring, ignite it again for secondary incineration; obtain the incineration slag after the secondary incineration.

[0075] Obtain incineration slag after secondary incineration, including:

[0076] Pour the incineration slag after secondary incineration into a ball mill for grinding;

[0077] Obtaining processed incineration slag, and placing the processed incineration slag on a vibrating screen for screening;

[0078] The particle size of the vibrating screen holes is controlled at 8 mm to obtain the sieved incineration slag;

[0079] Get freshly quenched garbage incineration slag in a sealed container, heat the sealed container to 110° C., and after heating for a period of time, force ventilation for weathering treatment, cycle heating and ventilation for 8 times, and get air-dried incineration slag for use;

[0080] S102: Weighing iron salt, zinc salt and ammonia monohydrate according to weight, grinding the iron salt and zinc salt, dissolving them in deionized water, and mechanically stirring for 8 minutes, and then titrating ammonia monohydrate into the mixed solution in sequence, adjusting the pH of the mixed solution to 10, and obtaining a mixed solution;

[0081] S103: placing the mixed solution into an autoclave, adjusting the temperature of the autoclave to 240° C. for reaction for 8 hours, and adjusting the temperature of the autoclave to 140° C. after the reaction is completed, tempering the product for 1 hour, and then cooling and drying to obtain an intermediate product of ferroferric oxide;

[0082] S104: adding the ferroferric oxide intermediate product to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, mixing well, and then adding ammonium sulfate to obtain a building block auxiliary material;

[0083] S105: placing the air-dried incineration slag in a mixing box, adding auxiliary building block materials and cement into the mixing box, stirring for 4 hours to make the mixture evenly mixed, and then introducing it into a brick press for pressing and molding. After pressing and molding and drying, lightweight building blocks are obtained.

[0084] In this embodiment, when the iron salt and the zinc salt are mixed with deionized water, the stirring speed of the stirrer is 2000 r / min, and the particle size of the iron salt and the zinc salt after being ground and crushed is 8 mm.

[0085] In this embodiment, the ferroferric oxide intermediate product is added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, mixed evenly and then ammonium sulfate is added, comprising:

[0086] The ferroferric oxide intermediate product was added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid and mechanically stirred for 13 minutes;

[0087] Continuously add ammonium sulfate to the mixed solution while stirring until the titration is completed and then stir for 13 minutes to obtain the building block auxiliary material.

[0088] In this embodiment, the internal temperature of the brick press is 120°C when pressing bricks.

[0089] Example 3

[0090] Reference Figure 1-2 As shown, a waste incineration slag treatment process specifically includes the following steps:

[0091] S1 01: Obtain the garbage to be incinerated and place it in an incinerator, perform preliminary draining, and perform a primary incineration after the preliminary draining is completed; after the primary incineration is completed, perform preliminary stirring on the garbage incineration slag, and after stirring, ignite it again for secondary incineration; obtain the incineration slag after the secondary incineration.

[0092] Obtain incineration slag after secondary incineration, including:

[0093] Pour the incineration slag after secondary incineration into a ball mill for grinding;

[0094] Obtaining processed incineration slag, and placing the processed incineration slag on a vibrating screen for screening;

[0095] The particle size of the vibrating screen is controlled at 10 mm to obtain the sieved incineration slag;

[0096] Get freshly quenched garbage incineration slag in a sealed container, heat the sealed container to 120° C., and after heating for a period of time, force ventilation for weathering treatment, cycle heating and ventilation for 10 times, and get air-dried incineration slag for use;

[0097] S102: Weighing iron salt, zinc salt and ammonia monohydrate according to weight, grinding the iron salt and zinc salt, dissolving them in deionized water, and mechanically stirring for 10 minutes, and then titrating ammonia monohydrate into the mixed solution in sequence, adjusting the pH of the mixed solution to 11, and obtaining a mixed solution;

[0098] S103: placing the mixed solution into an autoclave, adjusting the temperature of the autoclave to 250° C. for reaction for 10 h, and adjusting the temperature of the autoclave to 150° C. after the reaction is completed, tempering the product for 2 h, and then cooling and drying to obtain an intermediate product of ferroferric oxide;

[0099] S104: adding the ferroferric oxide intermediate product to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, mixing well, and then adding ammonium sulfate to obtain a building block auxiliary material;

[0100] S105: placing the air-dried incineration slag in a mixing box, adding auxiliary building block materials and cement into the mixing box, stirring for 5 hours to make the mixture evenly mixed, and then introducing it into a brick press for pressing and molding. After pressing and molding and drying, lightweight building blocks are obtained.

[0101] In this embodiment, when the iron salt and the zinc salt are mixed with deionized water, the stirring speed of the stirrer is 2200 r / min, and the particle size of the iron salt and the zinc salt after being ground and crushed is 10 mm.

[0102] In this embodiment, the ferroferric oxide intermediate product is added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, mixed evenly and then ammonium sulfate is added, comprising:

[0103] The ferroferric oxide intermediate product was added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid and mechanically stirred for 15 minutes;

[0104] Continuously add ammonium sulfate to the mixed solution while stirring until the titration is complete and then stir for 15 minutes to obtain the building block auxiliary material.

[0105] In this embodiment, the internal temperature of the brick press is 130°C when pressing bricks.

[0106] Comparison example

[0107] The lightweight blocks prepared in Examples 1-3 are now compared with existing lightweight concrete blocks (control examples). The comparison results are shown in the following table (at room temperature):

[0108]

[0109]

[0110] It can be seen from the above table that the concrete blocks manufactured by the present invention are 3KN / m3 lighter than the control example, and the compressive strength is increased by 25%. Compared with the ordinary concrete lightweight blocks, the weight is reduced by 5-10%, and the pores of the foam-like porous structure are irregularly distributed, resulting in the adsorption of the incineration slag and the complex phase, thereby enhancing its bonding force. Specifically, the compressive strength is enhanced by more than 30%. Since the ferroferric oxide has unique electrical and magnetic properties, when zinc is added, the particle size of the zinc-doped ferroferric oxide obtained is reduced, the dispersion is increased, the specific surface area is increased, and the saturation magnetization of the ferroferric oxide is increased, the coercive force is reduced, and it is beneficial to improve The magnetic loss capacity of ferroferric oxide is enhanced. During polymerization, aniline monomers will first polymerize on the surface of zinc-doped ferroferric oxide particles. Since the prepared zinc-doped ferroferric oxide has good dispersibility, the polymers formed at the beginning are separated from each other; as the polymerization reaction proceeds, the mutual entanglement of polyaniline molecular chains makes it impossible for the formed conductive polyaniline to be completely separated from each other, thus eventually forming a foam-like porous structure and a complex with irregular pore distribution, which is then combined with incineration slag and cement, resulting in adsorption of the incineration slag and the complex, thereby enhancing its bonding force. At the same time, the degradation of residual organic matter in the weathered slag will also form new pores, making the formed lightweight blocks lighter.

[0111] Reference Figure 3-5As shown, the present embodiment also discloses a waste incineration slag treatment system, which executes the above-mentioned waste incineration slag treatment process. The treatment system includes: a monitoring module, which is used to monitor the execution equipment of the waste incineration slag treatment process throughout the process to ensure that each treatment process meets the requirements for treatment; an MCU module, which is used to issue and terminate instructions to the execution equipment of the waste incineration slag treatment process, and realize each process link. The MCU module controls the corresponding execution equipment to complete the corresponding action output, and after the action is executed, it issues a termination signal to the execution equipment to enter the standby mode.

[0112] In this embodiment, the execution equipment includes: an incinerator for obtaining freshly quenched waste incineration slag; a closed container for heating and weathering the obtained freshly quenched waste incineration slag to remove excess moisture in the waste incineration slag; an autoclave for high-pressure heating of the mixed liquid to obtain an intermediate product of ferroferric oxide; a mixing box for mixing the air-dried incineration slag with auxiliary block materials and cement to form a lightweight block pre-processed material; a brick press for pressing and molding the formed lightweight block pre-processed material to obtain a lightweight block after pressing, molding and drying.

[0113] In this embodiment, the incinerator includes an incinerator and a stirring mechanism. The incinerator is used to incinerate the material in the incinerator. The monitoring module stops the incineration operation when it detects that the combustion in the incinerator is completed, and sends a signal to the stirring mechanism. The stirring mechanism stirs the material after the first incineration is completed. After the stirring is completed, the signal is fed back to the incinerator. The incinerator performs a second incineration on the material in the incinerator to ensure that the incineration is more comprehensive. During weathering, only a maximum of 5% of the organic matter is oxidized to form a hollow body.

[0114] In this embodiment, the monitoring module includes: a first monitoring unit, which is used to monitor the incineration state of garbage in the incinerator, and obtain the progress of garbage incineration by monitoring the smoke concentration generated during incineration and the internal temperature; a second monitoring unit, which is used to monitor whether the temperature in the closed container reaches a preset temperature; a third monitoring unit, which is used to monitor whether the reaction temperature in the autoclave reaches a preset temperature; a fourth monitoring unit, which is used to monitor the mixing time of the mixing box, and send a signal to the MCU module after the mixing time is reached, and the MCU module sends a mixing termination signal to the mixing box; a fifth monitoring unit, which is used to monitor whether the mixing time of the mixing box reaches a preset temperature ... The fifth monitoring unit is used to monitor whether the internal temperature of the brick press reaches the preset temperature when pressing bricks; the alarm unit is used to confirm the data monitored by the first monitoring unit, the second monitoring unit, the third monitoring unit and the fifth monitoring unit. If the preset conditions are not met, the alarm function is executed. The whole process is monitored through the monitoring module to ensure that the system processes the garbage slag according to the preset values, so that the foamy porous structure complex is easy to mix with cement, and the cement adheres to the surface of the incineration slag, so that the incineration slag and the block auxiliary materials are more tightly bonded, so as to improve the strength of the generated lightweight blocks, thereby greatly reducing the production cost of construction.

[0115] The technical solution generates zinc-doped ferroferric oxide through the reaction of iron salt and zinc salt. Due to the dual effects of static electricity and hydrogen bonds, the bonding force between the ferroferric oxide and aniline is enhanced, and finally a foamy porous structure is formed with a lighter weight, thereby reducing the weight of the prepared concrete blocks. Compared with ordinary concrete blocks, the weight is reduced by 5-10%, and the pores of the foamy porous structure are irregularly distributed, resulting in adsorption of the incineration slag and the complex phase, thereby enhancing its bonding force. At the same time, the degradation of residual organic matter in the weathered slag will also form new pores, making the formed lightweight blocks lighter.

[0116] In this embodiment, the entire operation process can be controlled by a computer, and with the addition of a PLC, etc., automated operation control can be achieved. In each operation link, sensors can be set up to provide signal feedback to achieve sequential execution of steps. These are all common knowledge of current automated control and will not be described in detail in this embodiment.

[0117] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A waste incineration slag treatment process, It is characterized in that The specific steps include: S101: freshly quenched waste incineration slag is obtained in a sealed container, and the sealed container is heated to 100-120° C. After heating for a period of time, forced ventilation is performed for weathering treatment, and the heating and ventilation cycle is repeated 5-10 times to obtain air-dried incineration slag for use; S102: Weighing iron salt, zinc salt and ammonia monohydrate by weight, grinding the iron salt and zinc salt, dissolving them in deionized water, and mechanically stirring for 5-10 minutes, and then titrating ammonia monohydrate into the mixed solution in sequence, adjusting the pH of the mixed solution to 9-11, and obtaining a mixed solution; S103: placing the mixed solution into an autoclave, adjusting the temperature of the autoclave to 230-250° C. for reaction for 5-10 hours, and adjusting the temperature of the autoclave to 130-150° C. after the reaction is completed, tempering the product for 1-2 hours, and then cooling and drying to obtain an intermediate product of ferroferric oxide; S104: adding the ferroferric oxide intermediate product to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, mixing well, and then adding ammonium sulfate to obtain a building block auxiliary material; S105: placing the air-dried incineration slag in a mixing box, adding auxiliary building block materials and cement into the mixing box, stirring for 3-5 hours to make the mixture evenly mixed, and then introducing it into a brick press for pressing and molding. After pressing and molding and drying, lightweight building blocks are obtained.

2. A process for treating waste incineration slag as claimed in claim 1, It is characterized in that In S101, freshly quenched waste incineration slag is obtained in a closed container, including: Obtain the garbage to be incinerated and place it in an incinerator for preliminary draining, and then incinerate it once after the preliminary draining is completed; After the first incineration is completed, the waste incineration slag is initially stirred, and then ignited again for secondary incineration; Obtain the incineration slag after secondary incineration.

3. A process for treating waste incineration slag as claimed in claim 2, It is characterized in that Obtain incineration slag after secondary incineration, including: Pour the incineration slag after secondary incineration into a ball mill for grinding; Obtaining processed incineration slag, and placing the processed incineration slag on a vibrating screen for screening; The particle size of the vibrating screen holes is controlled at 5-10 mm to obtain the sieved incineration slag.

4. A process for treating waste incineration slag as claimed in claim 3, It is characterized in that In S102, when the iron salt and the zinc salt are mixed with deionized water, the stirring speed of the stirrer is 1800-2200 r / min, and the particle size of the iron salt and the zinc salt after being ground and crushed is 5-10 mm.

5. A process for treating waste incineration slag as claimed in claim 4, It is characterized in that In S104, the ferroferric oxide intermediate product is added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid, and ammonium sulfate is added after mixing evenly, including: The ferroferric oxide intermediate product is added to a mixed solution of deionized water, aniline and concentrated hydrochloric acid and mechanically stirred for 10-15 minutes; Continuously add ammonium sulfate to the mixed solution while stirring until the titration is complete and then stir for 10-15 minutes to obtain the building block auxiliary material.

6. A process for treating waste incineration slag as claimed in claim 5, It is characterized in that In S105, the internal temperature of the brick press when pressing bricks is 110-130°C.

7. A waste incineration slag treatment system, It is characterized in that The waste incineration slag treatment process according to any one of claims 1 to 6 is implemented, wherein the treatment system comprises: The monitoring module is used to monitor the execution equipment of the waste incineration slag treatment process throughout the process to ensure that each treatment process meets the requirements; The MCU module is used to issue and terminate instructions to the execution equipment of the waste incineration slag treatment process to implement each process link. The MCU module controls the corresponding execution equipment to complete the corresponding action output, and after the action is completed, it issues a termination signal to the execution equipment to enter the standby mode.

8. A waste incineration slag treatment system as claimed in claim 7, It is characterized in that The execution device comprises: Incinerators for obtaining freshly quenched waste incinerator slag; A closed container is used to heat and weather the freshly quenched waste incineration slag to remove excess water from the waste incineration slag; An autoclave is used to heat the mixed solution under high pressure to obtain the intermediate product of ferroferric oxide; Mixing box, used to mix the air-dried incineration slag with auxiliary block materials and cement to form lightweight block pre-processing materials; The brick press is used to press and shape the pre-processed materials of the lightweight building blocks, and the lightweight building blocks are obtained after pressing, molding and drying.

9. A waste incineration slag treatment system as claimed in claim 8, It is characterized in that The incinerator includes an incinerator and a stirring mechanism. The incinerator is used to incinerate the material in the incinerator. The monitoring module stops the incineration operation when it detects that the combustion in the incinerator is completed, and sends a signal to the stirring mechanism. The stirring mechanism stirs the material after the first incineration is completed, and then feeds back a signal to the incinerator after the stirring is completed. The incinerator performs a second incineration on the material in the incinerator again.

10. A waste incineration slag treatment system as claimed in claim 9, It is characterized in that The monitoring module includes: A first monitoring unit, which is used to monitor the incineration state of the garbage in the incinerator, and obtain the progress of the garbage incineration by monitoring the smoke concentration generated during incineration and the internal temperature; A second monitoring unit, the second monitoring unit is used to determine whether the temperature in the sealed container reaches a preset temperature; A third monitoring unit, the third monitoring unit is used to monitor whether the reaction temperature in the autoclave reaches a preset temperature; A fourth monitoring unit, the fourth monitoring unit is used to monitor the boring mixing time in the mixing box, and send a signal to the MCU module after the mixing time is reached, and the MCU module then sends a mixing termination signal to the mixing box; A fifth monitoring unit, the fifth monitoring unit is used to monitor whether the internal temperature of the brick press reaches a preset temperature when pressing bricks; The alarm unit is used to confirm the data monitored by the first monitoring unit, the second monitoring unit, the third monitoring unit, and the fifth monitoring unit, and execute an alarm function if the preset conditions are not met.

Citation Information

Patent Citations

  • Method for processing household waste incineration slag

    CN107265899A

  • Porous zinc-doped ferriferrous oxide / polyaniline composite material

    CN107298762A

  • Method of using urban domestic waste incinerator residue to produce lightweight foam concrete

    CN109354448A

  • Transformer substation-based protective exterior wall

    CN109577701A

  • Device for manufacturing foam concrete by using incineration slag

    CN117901232A