Straight HRB635E high-strength twisted steel and rolling method thereof
By optimizing the heating process and rolling method, the problem of producing Φ50mm high-strength steel bars in the prior art was solved, and high-strength and low-cost production was achieved, ensuring that the size and performance of the steel bars meet the requirements.
Patent Information
- Application Number
- CN202411041283.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The prior art is difficult to produce Φ50mm high-strength steel bars that meet the needs of large high-rise buildings and large-span public buildings, and the cost is difficult to control during the production process, resulting in the difficulty of meeting the requirements at the same time.
By optimizing the heating process and rolling method of the billet, including controlling the temperature and time in the heating furnace, using alternating flat and vertical rolling mills for ten passes, and selecting the appropriate hole type and pressing during the rolling process The quantity controls the composition and heating temperature of the billet to ensure high strength and specifications of the steel bars.
It has achieved the production of Φ50mm large-sized high-strength threaded steel bars with yield strength ≥675MPa and tensile strength ≥850MPa, while reducing production costs and ensuring that the size and performance of the steel bars meet the requirements.
Smart Images

Figure CN118875015A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel section rolling, and in particular to a straight HRB635E high-strength threaded steel bar and a rolling method thereof. Background Art
[0002] High-strength steel bars refer to hot-rolled ribbed steel bars with a yield strength of 500MPa or above. Compared with ordinary steel bars, they have higher strength and better comprehensive performance, can withstand greater loads, and improve the seismic performance and safety of concrete structures. At present, straight threaded steel bars are mainly produced in Φ12-40mmHRB400E, and a small amount of Φ12-32mmHRB500E and HRB600E are produced. For large high-rise buildings and large-span public buildings, high-strength steel bars of 500MPa or above are preferred, and some key bridges and other buildings require large-size high-strength steel bars.
[0003] However, the strength of Φ50mm steel bars produced by the current small-size technology is difficult to meet the requirements, and the size that can meet the strength requirements cannot reach Φ50mm. Moreover, as the steel bar market environment continues to deteriorate, the pressure to reduce costs and increase efficiency is gradually increasing. While producing qualified high-strength steel bars with specifications reaching Φ50mm, it is also necessary to consider cost issues. Therefore, it is urgent to reasonably design the rolling method of Φ50mmHRB635E so that the products produced can meet the quality and performance requirements while minimizing costs. Summary of the invention
[0004] In view of the shortcomings of the above prior art, the present invention provides a straight HRB635E high-strength threaded steel bar and a rolling method thereof. The steel bar rolling method of the present invention has high strength, yield strength ReL≥675MPa, and tensile strength Rm≥850MPa; can produce large-size straight high-strength steel bars of Φ50mm; and effectively saves costs. It is specifically achieved through the following technologies.
[0005] A method for rolling straight HRB635E high-strength threaded steel bars comprises the following steps:
[0006] The steel billet heated in the heating furnace is rolled ten times to obtain the steel billet;
[0007] Among them, during the rolling process, the hole profiles of the first and second passes are both box-shaped holes, wherein the bite angle of the first pass is not greater than 26°, and the reduction is 45-50mm;
[0008] The hole shapes of the third to tenth passes are respectively elliptical holes or circular holes;
[0009] The reduction of the third to eighth passes is 30-40mm; the reduction of the ninth and tenth passes is 20-25mm;
[0010] The inner diameter d of the hole of the tenth pass is 48.5±0.8mm, the roller gap s is 3-4mm, the transverse rib height h is 3.2±1.2mm, and the transverse rib top width b is 2.3-2.5mm.
[0011] The choice of hole type in hole design is very important, especially for finished holes. Improper size design will result in the size not meeting the requirements and the negative difference cannot be rolled out, that is, the actual weight is greater than the theoretical weight, resulting in increased costs.
[0012] Furthermore, the heating temperature and time of the heating furnace are: preheating section temperature ≤ 950°C, heating section temperature 1215-1240°C, soaking section temperature 1205-1240°C, and heating time ≥ 100 min.
[0013] Furthermore, the rolling mills from the first pass to the tenth pass are alternating flat rolling mills and vertical rolling mills.
[0014] Furthermore, in the tenth pass, the milling groove depth is 3.0-3.4 mm.
[0015] Furthermore, in the tenth pass, the transverse rib spacing is 16±1.0 mm.
[0016] Furthermore, in the tenth pass, the included angle between the transverse rib and the axis is 63°-67°, and the transverse rib oblique angle is 47°-48°.
[0017] Further, the hole types from the third pass to the tenth pass are alternately set to be elliptical holes and circular holes.
[0018] Further, the steel billet includes the following elements in weight percentage: C 0.26-0.28%, Si 0.65-0.80%, Mn 1.50-1.60%, V 0.165-0.175%, P≤0.035%, S≤0.035%, Nb 0.013-0.020%, and carbon equivalent Ceq 0.56-0.58%.
[0019] Under the same billet specifications, as the rolling specifications increase, the compression ratio of the rolled piece decreases and the steel bar strength becomes lower. Therefore, for billets with the same composition, performance inconsistencies are more likely to occur when rolling larger specifications.
[0020] During the heating stage of the heating furnace, a long heating temperature or a heating temperature that is too high will cause coarse original austenite grains, while a temperature that is too low or a heating time that is too short will affect the phase transformation and the uniformity of the diffusion of alloy elements, thereby affecting the performance of the steel bar. Therefore, it is very important to design the heating process reasonably.
[0021] In addition, in order to solve the problem that the temperature difference among the head, middle and tail of the steel billet is large (about 60°C), which leads to large performance differences among the same steel strip, the present invention has made the following improvements: the heating load of the preheating section is reduced, and the temperature of the preheating section is optimized from the original ≤1050°C to ≤950°C, thereby increasing the heating load of the heating section and the equalizing section, increasing the gas volume, and lengthening the combustion flame, so as to control the temperature difference among the head, middle and tail of the steel billet within 30°C.
[0022] A straight HRB635E high-strength threaded steel bar is prepared by the above rolling method.
[0023] Straight high-strength threaded steel bars usually adopt micro-alloying technology, which uses the addition of niobium, vanadium, etc. to form niobium and vanadium carbides and nitrides that precipitate in the steel, achieving the purpose of grain refinement and precipitation strengthening, thereby improving the performance of the steel bars.
[0024] Nb is a strong carbonitride-forming element, which can refine grains and strengthen by precipitation by dissolving in the matrix. However, the precipitation temperature of Nb carbonitride is higher than that of V, and the precipitation strengthening effect is often not obvious during the steel bar rolling process. In addition, if the Nb content is too high, the risk of cracking of the rolled piece will increase.
[0025] V is the most important alloying element in 600MPa grade high-strength steel bars. It can effectively improve the strength of steel bars through precipitation strengthening, solid solution strengthening and fine grain strengthening, and can make full use of cheap N elements, which is a more economical micro-alloying method.
[0026] C dissolves in the matrix and can significantly improve the strength of the steel bar through solid solution strengthening. It can also combine with strong carbide-forming elements to form carbides, playing a role in fine grain strengthening and precipitation strengthening. On the other hand, C significantly improves the hardenability of steel bars. Too high a content will cause bainite or martensite to appear in the structure, reduce the plasticity of the steel bar, and deteriorate the welding performance of the steel bar. In order to ensure good comprehensive performance, the C content of 600MPa high-strength steel bars can be designed to be within the range of 0.22%-0.28%.
[0027] Si can improve strength through solid solution strengthening, which is beneficial to improve the elastic limit and yield strength of steel bars. It is also an important deoxidizer. Si can also promote the precipitation of vanadium carbide (VC) and strengthen the precipitation effect of vanadium (V). The Si content of 600MPa grade high-strength steel bars can be designed within the range of 0.40%-0.80%.
[0028] Mn can significantly improve the tensile strength of steel bars, but it also improves hardenability. When the Mn content exceeds 1.5%, abnormal structures of steel bars are likely to occur, which is unfavorable for ductility and weldability. The Mn content also affects the precipitation of vanadium nitride (VN). The higher the Mn content, the less VN content is precipitated. Therefore, the appropriate Mn content control range is 1.30%-1.60%. In the rolling method of the present invention, the Mn content in the steel billet can be controlled at 1.50-1.60%.
[0029] P and S are both harmful elements. When the P and S content is high, the plasticity and toughness of the steel bars will be reduced, cracks will easily occur during the rolling process, and it is also harmful to the welding and cold bending properties. When designing the composition, the upper limit values of P and S should be reduced as much as possible according to the actual production conditions.
[0030] Furthermore, the specification of the steel bar is Φ50mm.
[0031] Furthermore, the yield strength of the steel bar ReL≥675MPa, the tensile strength Rm≥850MPa, the maximum force total elongation Agt≥9.5%, R°m / R°eL≥1.26, and R°eL / ReL≤1.08.
[0032] Compared with the prior art, the present invention is beneficial in that:
[0033] 1. The composition control combined with the rolling method of the present invention can produce a large-size threaded steel bar of Φ50mm, and the yield strength ReL of the steel bar is ≥675MPa, the tensile strength Rm is ≥850MPa, the maximum force total elongation Agt is ≥9.5%, R°m / R°eL is ≥1.26, and R°eL / ReL is ≤1.08;
[0034] 2. The rolling method of the present invention controls the heating temperature and time so that the temperature difference between the head, middle and tail of the steel billet is within 30°C, thus maintaining the stability of the performance of the same steel bar;
[0035] 3. The hole type design of the tenth pass finished hole of the present invention is reasonable, and the size of the rolled finished product not only meets the requirements, but also the actual weight is less than the theoretical weight, thus achieving the goal of cost reduction. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the cross-sectional view of the finished hole of the tenth pass;
[0037] Figure 2 This is the cross-sectional view of the transverse rib after the tenth milling pass;
[0038] Figure 3 This is the longitudinal section of the tenth finished hole. DETAILED DESCRIPTION
[0039] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0040] The present invention provides an exemplary method for rolling straight HRB635E high-strength threaded steel bars, comprising the following steps:
[0041] The steel billet is heated in a heating furnace and then rolled ten times to obtain the straight HRB635E high-strength threaded steel bar of the present invention;
[0042] Among them, during the rolling process, the hole profiles of the first and second passes are both box-shaped holes, wherein the bite angle of the first pass is not greater than 26°, and the reduction is 45-50mm;
[0043] The hole shapes of the third to tenth passes are oval holes or circular holes, respectively, and the pressing amount of the third to eighth passes is 30-40mm; the pressing amount of the ninth and tenth passes is 20-25mm;
[0044] The inner diameter d of the hole of the tenth pass is 48.5±0.8mm, the roller gap s is 3-4mm, the transverse rib height h is 3.2±1.2mm, and the transverse rib top width b is 2.3-2.5mm.
[0045] In some examples of the present invention, the heating temperature and time of the heating furnace can be: preheating section temperature ≤ 950°C, heating section temperature 1215-1240°C, soaking section temperature 1205-1240°C, and heating time ≥ 100 min.
[0046] In some examples of the present invention, the rolling mills from the first pass to the tenth pass may be alternating between flat rolling mills and vertical rolling mills.
[0047] In order to facilitate the groove removal during rolling and reduce the failure of the guard plate wrapping around the roller, in some examples of the present invention, in the tenth pass, the milling groove depth can be 3.0-3.4 mm.
[0048] In order to extend the service life of the roller, in some examples of the present invention, in the tenth pass, the transverse rib spacing L may be 16±1.0 mm.
[0049] In order to facilitate the groove removal of the rolled piece, in some examples of the present invention, in the tenth pass, the angle β between the transverse rib and the axis can be 63°-67°, and the transverse rib oblique angle α can be 47°-48°.
[0050] In some examples of the present invention, the hole shapes from the third pass to the tenth pass may be alternately arranged as elliptical holes and circular holes.
[0051] In some examples of the present invention, the steel billet may include the following elements in weight percentage: C 0.26-0.28%, Si 0.65-0.80%, Mn 1.50-1.60%, V 0.165-0.175%, P≤0.035%, S≤0.035%, Nb 0.013-0.020%, and carbon equivalent Ceq 0.56-0.58%.
[0052] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] In some examples of the present invention, the rolling mills of ten passes are numbered 1#, 2#, 3#, 4#, 5#, 6#, 7#, 8#, 9#, and 10# respectively.
[0054] In some examples of the present invention, according to the finished product size requirements, the pressing amount of each pass is allocated according to the total deformation amount:.
[0055] The hole type of 1# and 2# adopts box-shaped hole, and the rolling deformation is achieved by large reduction. 1# is the first pass, and the problem of smooth bite needs to be considered. The bite angle is not greater than 26°, and the reduction of 1# and 2# is set to 45-50mm;
[0056] The hole types from 3# to 10# alternate between elliptical holes and circular holes, and a small reduction is used to control the width to ensure stable rolling and that the rolled piece size meets the requirements. Among them, the reduction of 3#, 4#, 5#, 6#, 7#, and 8# are all 30-40mm; the reduction of 9# and 10# are both 20-25mm.
[0057] The maximum reduction can be calculated according to the formula of reduction △h=D(1-cosα) (D is the working roller diameter of the roller, that is, the diameter of the working surface of the roller). In the present invention, the width expansion coefficient (=△b / △h, △b is the width deformation) is about 0.25-0.55, the width expansion coefficient of the 1# box hole is 0.27, and the width expansion of the 1# rolled piece can be calculated; in 3#-10#, the width expansion coefficient of the elliptical hole is 0.4-0.5, and the width expansion coefficient of the round hole is 0.3-0.4. The size of the rolled piece in each pass can be calculated by combining the width expansion coefficient of each pass.
[0058] Example 1
[0059] The method for rolling straight HRB635E high-strength threaded steel bars provided in this embodiment comprises the following steps:
[0060] S1. Acceptance of steel billet composition. 162mm×162mm HRB635E steel billet includes the following elements by weight percentage: C0.27%, Si 0.67%, Mn 1.55%, V 0.169%, P 0.022%, S 0.027%, Nb 0.016, carbon equivalent Ceq 0.57%; and visually inspect each steel billet to confirm that the section, shape, size, surface quality, etc. meet the specified requirements;
[0061] S2. The steel billet of step S1 is placed in a heating furnace for heating. The temperatures of the heating furnace are: 925°C in the preheating section, 1225°C in the heating section, and 1220°C in the soaking section. The heating furnace is automatically controlled in temperature. The furnace time is strictly controlled to be 103 minutes to allow the alloy elements to be fully dissolved and diffused. While ensuring the furnace temperature, the heating section and the soaking section adopt a high heat load mode to increase the flame length.
[0062] S3, rolling the steel billet of step S2 by ten passes to obtain the straight HRB635E high-strength threaded steel bar of the present invention;
[0063] In this embodiment, if Figure 1-3 As shown, the circular hole of the tenth pass is a finished hole, with an inner diameter d of 48.3 mm, a transverse rib height h of 3 mm, a transverse rib top width b of 2.3 mm, a transverse rib spacing L of 16.3 mm, an angle β between the transverse rib and the axis of 65°, and a transverse rib bevel angle α of 47.5°; the rolling parameter settings of each pass are shown in Table 1.
[0064] Table 1 Rolling parameter settings for each pass
[0065]
[0066] The applicant has conducted a large number of experiments within the range of the elements of the steel billet composition, the heating furnace parameters and the rolling parameters of the present invention, and found that the straight HRB635E high-strength threaded steel bar of the present invention can be prepared. The temperature of the steel billet at the inlet of the 9# rolling mill in step S2 is basically controlled at 1120-1150°C, and the temperature difference between the head, middle and tail of the steel billet is 30°C.
[0067] Example 2
[0068] This embodiment is substantially the same as Embodiment 1, except that the steel billet in this embodiment includes the following elements in weight percentage: C 0.27%, Si 0.69%, Mn 1.56%, V 0.168%, P 0.031%, S 0.033%, Nb 0.015, and carbon equivalent Ceq 0.57%.
[0069] Comparative Example 1
[0070] This comparative example is basically the same as Example 1, except that the steel billet in this comparative example includes the following elements in weight percentage: C 0.27%, Si 0.67%, Mn 1.55%, V 0.149%, P 0.022%, S 0.027%, Nb 0.016, and carbon equivalent Ceq 0.57%.
[0071] That is, in the steel billet of this comparative example, the weight percentage of V is lower than the range of the present invention.
[0072] Comparative Example 2
[0073] This comparative example is basically the same as Example 1, except that the inner diameter d of the finished hole of the tenth pass of the rolling mill in this comparative example is 49.5 mm.
[0074] That is, the inner diameter d of the finished hole of the tenth pass of the rolling mill in this comparative example exceeds the scope of the present invention.
[0075] Comparative Example 3
[0076] This comparative example is basically the same as Example 1, except that in this comparative example, the transverse rib height h of the finished hole of the tenth pass of the rolling mill is 4.5 mm.
[0077] That is, the transverse rib height h of the finished hole of the tenth rolling mill in this comparative example exceeds the scope of the present invention.
[0078] Application Examples
[0079] The steel bars of Examples 1-2 and Comparative Examples 1-3 were sized and tested for performance according to the method of "Steel for reinforced concrete Part 2: Hot-rolled ribbed steel bars" (GB / T 1499.2-2018). The dimensional measurement results and performance test results are shown in Table 2 below.
[0080] Table 2 Steel bar (HRB635E) dimension measurement and performance test results
[0081]
[0082] In Table 2, ReL represents the standard requirement value, which is 635MPa. R°m is the measured tensile strength of the steel bar; R°eL is the measured lower yield strength of the steel bar.
[0083] In the present invention, the quality inspection standards are: yield strength ReL≥635MPa, tensile strength Rm≥795MPa, maximum force total elongation Agt≥9.0%, R°m / R°eL≥1.25, R°eL / ReL≤1.30.
[0084] It can be seen from Table 2 that Examples 1-2 can stably prepare HRB635E threaded steel bars with a large size of 50 mm, and the steel bar yield strength ReL≥675 MPa, tensile strength Rm≥850 MPa, maximum force total elongation Agt≥9.5%, R°m / R°eL≥1.26, and R°eL / ReL≤1.08.
[0085] Compared with Example 1, the performance or finished product size and negative difference of Comparative Examples 1-3 do not meet the requirements. The yield strength of the steel bar in Comparative Example 1 does not meet the requirements. The negative difference of the steel bar in Comparative Example 2 does not meet the requirements. The inner diameter of the steel bar in Comparative Example 3 is too small and does not meet the requirements. In Comparative Example 3, the height of the transverse rib is relatively high, and the transverse rib is difficult to be removed from the groove, resulting in steel blocking.
[0086] The above specific embodiments describe the implementation of the present invention in detail, but the present invention is not limited to the specific details in the above embodiments. Within the scope of the claims and technical concept of the present invention, the technical solution of the present invention can be modified and changed in many simple ways, and these simple modifications all belong to the protection scope of the present invention.
Claims
1. A method for rolling straight HRB635E high-strength threaded steel bars, characterized in that: The following steps are involved: The steel billet heated in the heating furnace is rolled through ten passes to obtain the steel billet; Among them, during the rolling process, the hole profiles of the first and second passes are both box-shaped holes, wherein the bite angle of the first pass is not greater than 26°, and the reduction is 45-50mm; The hole shapes of the third to ninth passes are respectively elliptical holes or circular holes; The reduction of the third to eighth passes is 30-40mm; the reduction of the ninth and tenth passes is 20-25mm; The inner diameter of the circular hole of the tenth pass is 48.5±0.8mm, the roller gap is 3-4mm, the cross rib height is 3.2±1.2mm, and the cross rib top width is 2.3-2.5mm.
2. The rolling method according to claim 1, characterized in that: The steel billet comprises the following elements in weight percentage: C 0.26-0.28%, Si 0.65-0.80%, Mn 1.50-1.60%, V 0.165-0.175%, P≤0.035%, S≤0.035%, Nb 0.013-0.020%, and carbon equivalent Ceq 0.56-0.58%.
3. The rolling method according to claim 1, characterized in that: The heating temperature and time of the heating furnace are: preheating section temperature ≤950°C, heating section temperature 1215-1240°C, soaking section temperature 1205-1240°C, and heating time ≥100min.
4. The rolling method according to claim 1, characterized in that: The rolling mills from the first pass to the tenth pass are alternately flat rolling mills and vertical rolling mills.
5. The rolling method according to claim 1, characterized in that: In the tenth pass, the milling groove depth is 3.0-3.4 mm.
6. The rolling method according to claim 1, characterized in that: In the tenth pass, the transverse rib spacing is 16±1.0 mm.
7. The rolling method according to claim 1, characterized in that: In the tenth pass, the included angle between the transverse rib and the axis is 63°-67°, and the transverse rib oblique angle is 47°-48°.
8. The rolling method according to claim 1, characterized in that: The hole shapes of the third to tenth passes are alternately arranged to be elliptical holes and circular holes.
9. A straight HRB635E high-strength threaded steel bar, characterized in that: The steel sheet is prepared by the rolling method described in any one of claims 1 to 8.
10. The straight HRB635E high-strength threaded steel bar according to claim 9, characterized in that: The specification of the steel bar is Φ50mm.
Citation Information
Patent Citations
Method for producing large-specification circular blanks in rolling mode instead of forging mode
CN108356073A
Stainless steel composite steel bar and preparation method thereof
CN113877961A
Negative deviation comprehensive control method for HRB500E deformed steel bar
CN115213234A
Finish rolling pass system and rolling method for stainless steel composite twisted steel and stainless steel composite twisted steel
CN116673337A
Rolling method for hot rolled steel plate
JP2016078026A