Production method capable of avoiding oriented silicon steel hot rolling hemming cracks

Through continuous casting of chamfer crystallizers and controlling heating conditions, the rolling process is optimized, and the problem of hot-rolled coil edge cracks of oriented silicon steel is solved, the material yield and edge quality are improved, and more efficient hot-rolled coil production is achieved.

CN119056869AActive Publication Date: 2024-12-03HUNAN VALIN LIANYUAN IRON & STEEL CO LTD +1

Patent Information

Application Number
CN202411328187.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

Oriented silicon steels are prone to edge crack defects during hot rolling, resulting in a decrease in material yield, and it is difficult for the prior art to effectively avoid this problem.

Method used

Continuous casting of the casting billet is obtained by chamfering crystallizer, and the surface temperature is controlled to be no less than 400°C in the heating furnace. Heating is performed using a reducing atmosphere. The rolling process is optimized to reduce edge decarbonization and coarse grains, and improve the plate. The blank shape is to slow down heat dissipation and reduce the temperature drop rate.

Benefits of technology

The edge crack defects of oriented silicon steel hot-rolled coils are effectively avoided, the material yield and edge quality are improved, the hot-rolling cutting loss is reduced, and the overall performance of the product is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056869A_ABST
    Figure CN119056869A_ABST
Patent Text Reader

Abstract

The invention discloses a production method capable of avoiding oriented silicon steel hot rolling hemming cracks. The method comprises the following steps: continuously casting molten steel through a chamfering crystallizer to obtain a casting blank; the surface temperature of the casting blank before entering the heating furnace is not lower than 400 DEG C; the casting blank is heated in a heating furnace, the furnace gas temperature ranges from 1100 DEG C to 1330 DEG C, the atmosphere in the furnace is a reducing atmosphere, the total in-furnace time ranges from 200 min to 330 min, and a heated plate blank is obtained; and the heated plate blank is rolled and coiled, and the oriented silicon steel hot-rolled coil is obtained. According to the production method, the edge crack defect in the hot rolling process of the oriented silicon steel slab can be greatly improved, the edge quality of the oriented silicon steel is improved, and the yield of the oriented silicon steel is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of oriented silicon steel preparation, and specifically relates to a production method for preventing hot-rolled curling edge cracking of oriented silicon steel. Background Art

[0002] Grain-oriented silicon steel has excellent magnetic properties and is mainly used in power systems to achieve efficient electromagnetic conversion. It is mainly used to manufacture transformer cores. Through its excellent soft magnetic characteristics and magnetization properties, it provides high magnetic flux for transformers, thereby achieving efficient electric-magnetic-electric conversion functions.

[0003] The silicon content is very sensitive to the magnetic properties of oriented silicon steel. With the increase of silicon content, the resistivity increases, the eddy current loss decreases, and the iron loss also decreases. However, with the increase of silicon content, it has the characteristics of low high temperature strength, high low temperature strength, low thermal conductivity, and brittle performance. During the heating process of the slab, microcracks are easy to appear on the edge. During the hot rolling process of the oriented silicon steel slab with microcracks, under the action of the rolling force, the microcracks continue to expand and extend to the surface, and finally edge crack defects appear. Edge crack defects are prone to occur during hot rolling. Therefore, improvement is urgently needed. Summary of the invention

[0004] In view of this, the present application provides a production method for avoiding edge cracking of hot-rolled coils of oriented silicon steel, aiming to provide a production method that can significantly improve the edge cracking defects in the hot rolling process of oriented silicon steel slabs, improve the edge quality of oriented silicon steel, and improve the yield rate of oriented silicon steel.

[0005] In a first aspect, an embodiment of the present application provides a production method for preventing hot-rolled edge cracking of oriented silicon steel, comprising:

[0006] Continuous casting is carried out through a chamfered crystallizer to obtain a casting ingot;

[0007] The surface temperature of the ingot before entering the heating furnace is not less than 400℃;

[0008] The ingot is heated in a heating furnace, the furnace gas temperature is 1100°C-1330°C, the atmosphere in the furnace is a reducing atmosphere, and the total furnace time is 200-330 minutes to obtain a heated slab;

[0009] The heated slab is rolled and coiled to produce a oriented silicon steel hot rolled coil.

[0010] According to an embodiment of one aspect of the present application, the ingot includes the following chemical components by mass fraction: 0.03%≤C≤0.07%, 3.0%≤Si≤3.60%, 0.05%≤Mn≤0.30%, P≤0.03%, S≤0.011%, 0.015%≤Als≤0.032%, Cu≤0.6%, and the rest are iron and unavoidable trace elements.

[0011] According to an embodiment of one aspect of the present application, the transfer time between the cast billet from the continuous casting line and the heating furnace is 0h to 12h, so that the surface temperature of the cast billet before entering the heating furnace is not less than 400°C.

[0012] According to an embodiment of one aspect of the present application, the ingot is placed in an insulation pit with a burner, and the transfer time from the insulation pit to the heating furnace is less than 30 minutes, so that the surface temperature of the ingot before entering the heating furnace is not lower than 400°C.

[0013] According to an embodiment of one aspect of the present application, the rolling includes 5 rough rolling passes, and the total reduction rate of the rough rolling is 80%-86%.

[0014] According to an embodiment of one aspect of the present application, the reduction rate of each of the five rough rolling passes is 25%-40%.

[0015] According to an embodiment of one aspect of the present application, the thickness of the cast billet is 200-240 mm.

[0016] According to an embodiment of one aspect of the present application, the thickness of the hot-rolled plate is 1.8-3 mm.

[0017] According to an embodiment of one aspect of the present application, the heating furnace has a heating rate of 6°C-10°C / min; and the pressure applied by vertical rollers to the two side walls along the length direction is 0 to 1000N.

[0018] In a second aspect, an embodiment of the present application provides a oriented silicon steel hot-rolled coil, which is produced by the production method of the first aspect.

[0019] This application has at least the following beneficial effects:

[0020] The production method provided in the present application optimizes the shape of the oriented silicon steel slab and prepares the original right-angle slab into a chamfered slab by continuous casting in a chamfered crystallizer, so as to slow down the heat dissipation of the edge and avoid a rapid temperature drop; the surface temperature of the cast slab before entering the heating furnace is not less than 400°C, and at the same time, by controlling the atmosphere in the heating furnace, the furnace gas temperature is 1100°C-1330°C, the atmosphere in the furnace is a reducing atmosphere, and the total time in the furnace is 200-330min, which comprehensively reduces the decarburization of the edge and the problem of coarse grains, thereby avoiding edge cracks in the oriented silicon steel hot-rolled coil and improving the product yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solution of the implementation regulations of this application, the following is a brief introduction to the drawings required for use in the embodiments of this application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0022] Figure 1 The appearance of the oriented silicon steel ingot of Comparative Example 1 of the present application is shown.

[0023] Figure 2 The appearance of the oriented silicon steel ingot of Example 1 of the present application is shown.

[0024] Figure 3 The quality appearance of the hot-rolled curling edge of the oriented silicon steel of comparative example 1 of the present application is shown.

[0025] Figure 4 The quality appearance of the hot-rolled curling edge of the oriented silicon steel of Example 1 of the present application is shown. DETAILED DESCRIPTION

[0026] In order to make the application purpose, technical solution and beneficial technical effect of this application clearer, the application is further described in detail below in conjunction with the embodiments. It should be understood that the implementation regulations described in this specification are only for explaining this application, not for limiting this application.

[0027] For simplicity, the present application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0028] In the description of the present application, it should be noted that, unless otherwise specified, “above” and “below” are inclusive of the number, and the “multiple” in “one or more” means two or more than two.

[0029] The above application content of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided through a series of embodiments, and these implementation regulations can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0030] In a first aspect, an embodiment of the present application provides a production method for preventing hot-rolled edge cracking of oriented silicon steel, the method comprising:

[0031] The molten steel is continuously cast through a chamfered crystallizer to obtain a casting ingot;

[0032] The surface temperature of the ingot before entering the heating furnace is not less than 400℃;

[0033] The ingot is heated in a heating furnace, the furnace gas temperature is 1100°C-1330°C, the atmosphere in the furnace is a reducing atmosphere, and the total furnace time is 200-330 minutes to obtain a heated slab;

[0034] The heated slab is rolled and coiled to produce a oriented silicon steel hot rolled coil.

[0035] Generally speaking, the silicon content of oriented silicon steel is generally between 2.5% and 4%, but as the silicon content increases, it has the characteristics of low high temperature strength, high low temperature strength, low thermal conductivity, and brittle performance. During the heating process of the slab, the edges are prone to decarburization, coarse grains, and other problems, resulting in microcracks. During the hot rolling process of oriented silicon steel slabs with microcracks, under the action of rolling force, the microcracks continue to expand and extend to the surface, and finally edge crack defects appear. Edge crack defects are prone to occur during hot rolling.

[0036] Research has found that the silicon content of oriented silicon steel is high, and the solid solubility of silicon in austenite is greater than that in ferrite. During the transformation from austenite to ferrite, silicon tends to segregate to the grain boundary, causing embrittlement of the grain boundary; on the other hand, the edge temperature of the steel strip drops rapidly during rolling, causing the elongation of the edge to be lower than that of the matrix; on the other hand, silicon reduces the austenite area, which easily leads to unevenness of hot-rolled grains. Generally speaking, edge trimming is required after hot rolling, so if the edge crack is slight, there is no effect, but if the edge crack is serious, it will cause excessive edge trimming and a significant reduction in the yield rate.

[0037] The method of the present application changes the edge shape of the slab from a right angle to a chamfer, thereby reducing heat dissipation and temperature drop, reducing decarburization, and selecting appropriate temperature and reducing atmosphere during the heating process, thereby avoiding the generation of edge cracks, improving the edge quality of oriented silicon steel, increasing the yield rate, and reducing the amount of hot rolling cutting loss.

[0038] The right angle of the slab edge is optimized to a chamfer, so that it changes from three-dimensional heat transfer to two-dimensional heat transfer, which fundamentally reduces the excessive temperature drop rate of the edge and reduces the probability of cracks. When the corner of the slab is a right angle, its heat transfer is three-dimensional heat transfer, heat dissipation is faster, temperature drop is faster, and cracks are prone to occur. When it is optimized to a chamfered shape, it dissipates heat more slowly, the temperature difference with the inside of the slab is smaller, and the specific surface area is smaller, so it is not easy to crack. When the atmosphere of the heating furnace is a reducing atmosphere, the reaction between oxygen in the heating furnace and carbon in the slab is reduced, thereby reducing the decarburization of the corners of the slab, and its chamfered shape can weaken the local decarburization reaction, reducing the probability of cracks.

[0039] The above method does not require additional edge heating of the slab, simplifies the complex heating and temperature rise system of the heating furnace, does not require edge heating of the hot-rolled plate, and reduces edge decarburization by controlling the atmosphere in the heating furnace, thereby further improving the edge quality of oriented silicon steel.

[0040] In some optional embodiments, the ingot comprises the following chemical composition by mass fraction: 0.03%≤C≤0.07%, 3.0%≤Si≤3.60%, 0.05%≤Mn≤0.30%, P≤0.03%, S≤0.011%, 0.015%≤Als≤0.032%, Cu≤0.6%, and the rest are iron and unavoidable trace elements.

[0041] According to the embodiments of the present application, the use of the above-mentioned elemental composition can, on the one hand, avoid the elements causing grain boundary segregation and embrittlement of the grain boundaries, and on the other hand, help to further reduce the austenite area, which easily leads to the unevenness of hot-rolled grains, thereby improving the edge quality.

[0042] In some optional embodiments, the transfer time between the cast billet from the continuous casting line and the heating furnace is 0 h to 12 h, so that the surface temperature of the cast billet before entering the heating furnace is not less than 400° C.

[0043] In some optional embodiments, the ingot is placed in a holding pit with a burner, and the transfer time from the holding pit to the heating furnace is less than 30 minutes, so that the surface temperature of the ingot before entering the heating furnace is not less than 400°C.

[0044] In some optional embodiments, in order to reduce edge cracks, the rolling includes 5 rough rolling passes, and the total reduction ratio of the rough rolling is 80%-86%. In some optional embodiments, the rolling includes 7 finish rolling passes.

[0045] In some optional embodiments, the reduction rate of each of the five rough rolling passes is 25%-40%. According to the embodiments of the present application, when the reduction rate is too high, greater than 40%, the deformation is concentrated in the surface layer of the metal, which may cause stress concentration and increase the risk of edge cracks. Too low a reduction rate, less than 25%, will lead to insufficient metal deformation, which may require a larger deformation amount in the subsequent rolling process, and will also cause edge cracking (edge ​​cracking). A reasonable reduction rate helps the metal to deform evenly, reduce stress concentration, and reduce the risk of edge cracking.

[0046] In some optional embodiments, the thickness of the ingot is 200-240 mm.

[0047] In some optional embodiments, the hot-rolled plate has a thickness of 1.8-3 mm.

[0048] In some optional embodiments, in order to further reduce edge cracks and improve edge quality, the heating furnace heating rate is 6°C-10°C / min; the pressure applied by the vertical rollers on the two side walls along the length direction is 0 to 1000N.

[0049] Grain-oriented silicon steel hot-rolled coil

[0050] In a second aspect, an embodiment of the present application provides a oriented silicon steel hot-rolled coil, which is produced by the production method of the first aspect.

[0051] According to the embodiment of the present application, the yield rate of the oriented silicon steel hot-rolled coil is greater than or equal to 96.5%, the edge quality is better, and the yield rate is increased by 0.8%-3%. The edge grain of the oriented silicon steel hot-rolled coil is between 30-35 microns, which is much smaller than the edge grain of 55-75 microns produced by the original method, avoiding edge cracking caused by coarse grains of the oriented silicon steel hot-rolled coil.

[0052] Example

[0053] The following examples describe the disclosure of the present application in more detail, and these examples are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations may be made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0054] Example 1

[0055] The present application provides a production method for preventing hot-rolled edge cracking of oriented silicon steel, the method comprising:

[0056] The oriented silicon steel ingot is obtained by continuous casting through a chamfered crystallizer, and the thickness of the ingot is 210 mm.

[0057] By making the transfer time between the ingot from the continuous casting line and the heating furnace 4 to 9 hours, the surface temperature of the oriented silicon steel ingot before entering the heating furnace is controlled at 460°C;

[0058] The ingot was heated in a heating furnace with a furnace gas temperature of 1145°C and a reducing atmosphere. The total furnace time was 310 minutes.

[0059] The rough rolling was performed in five passes, and the total reduction ratio of the rough rolling was 81.6%.

[0060] Finish rolling and curling are performed.

[0061] Example 2

[0062] The present application provides a production method for preventing hot-rolled edge cracking of oriented silicon steel, the method comprising:

[0063] The oriented silicon steel ingot is obtained by continuous casting through a chamfered crystallizer, and the thickness of the ingot is 232 mm.

[0064] By making the transfer time between the ingot from the continuous casting line and the heating furnace 6h to 11h, the surface temperature of the oriented silicon steel ingot before entering the heating furnace is controlled at 413℃;

[0065] The ingot was heated in a heating furnace with a furnace gas temperature of 1283°C and a reducing atmosphere. The total furnace time was 289 minutes.

[0066] The rough rolling was performed in five passes, and the total reduction ratio of the rough rolling was 83.8%.

[0067] Finish rolling and curling are performed.

[0068] Example 3

[0069] The present application provides a production method for preventing hot-rolled edge cracking of oriented silicon steel, the method comprising:

[0070] The oriented silicon steel ingot is obtained by continuous casting through a chamfered crystallizer, and the thickness of the ingot is 240 mm.

[0071] By making the transfer time between the ingot from the continuous casting line and the heating furnace 3h to 7h, the surface temperature of the oriented silicon steel ingot before entering the heating furnace is controlled at 510℃;

[0072] The ingot was heated in a heating furnace with a furnace gas temperature of 1345°C and a reducing atmosphere. The total furnace time was 270 min.

[0073] The rough rolling was performed in five passes, and the total reduction ratio of the rough rolling was 84.2%.

[0074] Finish rolling and curling are performed.

[0075] Example 4

[0076] The present application provides a production method for preventing hot-rolled edge cracking of oriented silicon steel, the method comprising:

[0077] The oriented silicon steel ingot is obtained by continuous casting through a chamfered crystallizer, and the thickness of the ingot is 240 mm.

[0078] By making the transfer time between the ingot from the continuous casting line and the heating furnace 2h to 7h, the surface temperature of the oriented silicon steel ingot before entering the heating furnace is controlled to be 536℃;

[0079] The ingot was heated in a heating furnace with a furnace gas temperature of 1315°C and a reducing atmosphere. The total furnace time was 320 min.

[0080] The rough rolling was performed in five passes, and the total reduction ratio of the rough rolling was 84.2%.

[0081] Finish rolling and curling are performed.

[0082] Example 5

[0083] The difference between this embodiment and embodiment 1 is that five rough rolling passes are performed, and the total reduction ratio of the rough rolling is 71.2%.

[0084] Comparative Example 1

[0085] The difference between this comparative example and Example 1 is that a right-angle crystallizer is used for continuous casting.

[0086] Comparative Example 2

[0087] The difference between this comparative example and Example 1 is that the transfer time between the cast billet from the continuous casting line and the heating furnace is set to 15 hours, and the surface temperature of the oriented silicon steel cast billet before entering the heating furnace is controlled to be 380°C.

[0088] Comparative Example 3

[0089] The difference between this comparative example and Example 1 is that the ingot is heated in a heating furnace, the furnace gas temperature is 1000° C., the furnace gas atmosphere is maintained as an oxidizing atmosphere, and the total time in the furnace is 180 min.

[0090] Comparative Example 4

[0091] The difference between this comparative example and Example 2 is that the furnace gas atmosphere is maintained as an oxidizing atmosphere.

[0092] Test Section

[0093] The hot rolled coils prepared in the examples and comparative examples were tested.

[0094] The evaluation criteria for the quality of hot-rolled coils are: the edges are neat and free of cracks, and the edge crack depth is less than 2mm for qualified products; the edges have serious notches or the edge crack depth is less than 2mm for defective or unqualified products.

[0095] The calculation formula of the yield rate is: yield rate = the mass of steel after trimming / the mass of steel before trimming * 100%

[0096] After trimming, the edges of the steel are neat and free of cracks, and the depth of the cracks on the edges is less than 2mm.

[0097] Table 1 Test results of edge quality and yield rate of the embodiments and comparative examples.

[0098]

[0099]

[0100] The above measured performance parameters are taken as average values.

[0101] Figure 1 Figure 1 The appearance of the oriented silicon steel ingot of comparative example 1 of the present application is shown, which illustrates that the oriented silicon steel ingot produced by the right-angle crystallizer used in comparative example 1 is right-angled, and the heat dissipation at the right angle is fast, which is easy to cause hot rolling curling cracks.

[0102] Figure 2 The appearance of the oriented silicon steel ingot of Example 1 of the present application is shown, which illustrates that the oriented silicon steel ingot produced by the chamfered crystallizer used in Comparative Example 1 is chamfered, and the heat dissipation at the chamfer is slower, which is beneficial to reduce the heat dissipation speed and reduce the temperature drop, and can avoid hot rolling curling cracks.

[0103] Figure 3 The quality appearance picture of the hot-rolled curling edge of the oriented silicon steel of comparative example 1 of the present application is shown, which illustrates that the quality of the hot-rolled curling edge of the oriented silicon steel prepared in comparative example 1 is poor and cracks are obvious.

[0104] Figure 4 The quality appearance diagram of the hot-rolled curling edge of the oriented silicon steel of Example 1 of the present application is shown, which illustrates that the hot-rolled curling edge of the oriented silicon steel prepared in Example 1 has good quality, without obvious cracks and micro cracks.

[0105] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto, and any familiarity with the present technology or replacement should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A production method for avoiding hot-rolled edge cracking of oriented silicon steel, characterized in that: The method comprises: The molten steel is continuously cast through a chamfered crystallizer to obtain a casting ingot; The surface temperature of the ingot before entering the heating furnace is not less than 400℃; The ingot is heated in a heating furnace, the furnace gas temperature is 1100°C-1330°C, the atmosphere in the furnace is a reducing atmosphere, and the total furnace time is 200-330 minutes to obtain a heated slab; The heated slab is rolled and coiled to produce a oriented silicon steel hot rolled coil.

2. The production method according to claim 1, characterized in that The ingot comprises the following chemical components by mass fraction: 0.03%≤C≤0.07%, 3.0%≤Si≤3.60%, 0.05%≤Mn≤0.30%, P≤0.03%, S≤0.011%, 0.015%≤Als≤0.032%, Cu≤0.6%, and the rest are iron and inevitable trace elements.

3. The production method according to claim 1, characterized in that The transfer time between the ingot and the heating furnace is set to 0 to 12 hours so that the surface temperature of the ingot before entering the heating furnace is not less than 400°C.

4. The production method according to claim 1, characterized in that By placing the ingot in a heat preservation pit with a burner, the transfer time from the heat preservation pit to the heating furnace is less than 30 minutes, so that the surface temperature of the ingot before entering the heating furnace is not less than 400°C.

5. The production method according to claim 1, characterized in that: The rolling process includes five rough rolling passes, and the total reduction rate of the rough rolling is 80%-86%.

6. The production method according to claim 1, characterized in that: The reduction rate of each of the five rough rolling passes is 25%-40%.

7. The production method according to claim 1, characterized in that: The thickness of the ingot is 200-240 mm.

8. The production method according to claim 1, characterized in that: The thickness of the hot-rolled plate is 1.8-3 mm.

9. The production method according to claim 1, characterized in that: The heating furnace has a heating rate of 6°C-10°C / min; the pressure applied by the vertical rollers on the two side walls along the length direction is 0 to 1000N.

10. A hot-rolled oriented silicon steel coil, characterized in that: The method is prepared by the production method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for controlling roll gap of vertical roll of hot continuous rolling mill

    CN108213089A

  • Medium-temperature common oriented silicon steel and preparation method thereof

    CN113458142A

  • Production method for controlling edge defects of high-silicon strip steel and strip steel product

    CN116984383A

  • Method for preparing oriented silicon steel and oriented silicon steel

    CN117758033A

  • Method for reducing edge sawtooth-shaped burr chain defect of hot-rolled oriented silicon steel

    CN118595183A

Cited By

  • Production method for reducing edge cracks of high-magnetic-induction oriented silicon steel

    CN119640013A

  • Production method for improving edge quality of silicon steel

    CN120861584A

  • A production method for improving the quality of the edge portion of silicon steel

    CN120861584B