Preparation method of high-purity ruthenium-based alloy target material
By coating ammonium chlororuthenate with a vacuum hot pressing sintering technology, the problems of low density and complex process of high-purity ruthenium-based alloy targets in the existing technology are solved, and high density and microstructure controllability are achieved. The preparation of ruthenium-based alloy targets reduces the difficulty and cost of the process.
Patent Information
- Application Number
- CN202411113855.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
AI Technical Summary
The existing high-purity ruthenium-based alloy target preparation process has problems such as low density, poor microstructure controllability, complex process flow and high cost, which cannot meet the needs of high-performance ruthenium-based alloy targets.
The surface of the alloyed element particles was coated with ammonium chlororuthenate by ball milling, and vacuum hot-press sintering was carried out after calcining and reducing treatment to prepare a high-purity ruthenium-based alloy target, which reduced the sintering temperature and increased the density.
The density improvement of the ruthenium-based alloy target, the controllability of the microstructure, the process difficulty and cost reduction of the process are achieved, and a high-purity ruthenium-based alloy target with high density and low oxygen content is prepared.
Smart Images

Figure CN118875285A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a high-purity ruthenium-based alloy target material, and belongs to the technical field of preparation of ruthenium-based alloy target materials. Background Art
[0002] At present, with the evolution of semiconductor components towards miniaturization, the requirements for the refinement of integrated circuits and chips are becoming more and more stringent; thus, the requirements for the performance of diffusion barriers in semiconductors (film uniformity, conductivity and mechanical properties, etc.) have become more stringent. Due to the improvement of the performance requirements of the diffusion barrier layer, researchers have been prompted to conduct a new round of research and development work on new target materials used for the diffusion barrier layer. At present, refractory metals are widely used in diffusion barrier film materials due to their high melting point, good thermal stability and good conductivity. Current research shows that alloy compounds and non-metallic compounds (such as nitrides, silicides and carbides) of refractory metals such as tantalum, ruthenium, tungsten, titanium and zirconium have good barrier properties, and are basically insoluble in copper and do not react, and can be used as diffusion barriers. These films can provide good barrier properties at a lower thickness and can also improve thermal stability. Among them, since ruthenium-based alloys are refractory metals, the preparation of ruthenium-based alloy targets is mainly carried out by powder metallurgy and casting.
[0003] For example, CN115537593A discloses a platinum-ruthenium alloy target material and its preparation method and application, wherein the preparation method comprises: melting platinum, ruthenium, vanadium and chromium, refining and pouring them in sequence to obtain a cast billet; hot forging, rolling and annealing the cast billet in sequence to obtain a platinum-ruthenium alloy target material. CN104032270A discloses a large-size ruthenium-based alloy sputtering target material and its preparation method, wherein the preparation method comprises: preparing ruthenium and other alloy elements into ruthenium-based alloy powder by gas atomization powder making process, and then sintering the ruthenium-based alloy powder into a ruthenium-based alloy target material by vacuum hot pressing or spark plasma sintering. CN104226999A discloses a tantalum-ruthenium alloy target material and a preparation method thereof. The preparation method comprises mixing tantalum hydride powder and ruthenium powder into a mixed powder, and then sintering the mixed powder by hot isostatic pressing to obtain a high-purity tantalum-ruthenium alloy target blank, and machining the high-purity tantalum-ruthenium alloy target blank and welding it to a back plate to obtain a tantalum-ruthenium alloy target material assembly.
[0004] At present, the preparation process of pure ruthenium and ruthenium-based alloy targets is mainly through smelting and powder metallurgy, which has problems such as low density, poor microstructure controllability, complex process flow and high cost, and therefore cannot meet the demand for high-performance ruthenium-based alloy targets. Summary of the invention
[0005] In order to solve the problems existing in the existing preparation of ruthenium-based alloy target materials, the present invention provides a method for preparing a high-purity ruthenium-based alloy target material, and the method specifically comprises the following steps:
[0006] (1) Ammonium chlororuthenate and alloying element spherical particles are ball-milled using polytetrafluoroethylene and zirconium oxide ball milling balls, so that ammonium chlororuthenate is coated on the surface of the alloying element spherical particles to obtain composite powder.
[0007] (2) The composite powder obtained in step (1) is subjected to calcination and reduction treatment.
[0008] (3) The composite powder treated in step (2) is subjected to vacuum hot pressing and sintering to obtain a ruthenium-based alloy target material blank.
[0009] Preferably, in step (1), polytetrafluoroethylene and zirconium oxide ball milling balls are used for ball milling.
[0010] Preferably, the purity of the ammonium chlororuthenate in step (1) is 99.99%.
[0011] Preferably, the spherical particles of the alloying element in step (1) are tantalum, chromium or tungsten.
[0012] Preferably, the spherical particles of the alloying element in step (1) have a particle size of 10 to 30 μm and a purity of 99.99%.
[0013] Preferably, the atomic content percentage of the alloy element in the composite powder of step (1) is 1% to 30%, the remainder is ruthenium, and the total atomic percentage of the alloy element and ruthenium in the composite powder is 100%.
[0014] Preferably, the ball milling time in step (1) is 3 to 12 hours, the ball milling speed is 300 r / min, and the ball milling process is in a vacuum atmosphere.
[0015] Preferably, in step (2), the calcination temperature of the composite powder is 450-750° C., the time is 2-5 h, and the calcination environment is vacuum; the reduction temperature is 500-800° C., the time is 3-6 h, and the reducing atmosphere is an argon-hydrogen mixed atmosphere.
[0016] Preferably, during the vacuum hot pressing sintering in step (3), the sintering temperature is 1100-1300° C. and the holding time is 3 h to 6 h.
[0017] Beneficial effects of the present invention
[0018] (1) The present invention adopts a ball milling method to coat ammonium chlororuthenate on the surface of alloying element particles, so that the pure ruthenium particles decomposed and reduced can be made finer, thereby resulting in high surface sintering activity and reducing the sintering temperature of the ruthenium-based alloy target blank from the existing 1500°C to 1100°C, thereby further improving the density of the prepared ruthenium-based alloy target blank; at the same time, the fine pure ruthenium particles decomposed and reduced are conducive to reducing the overall grain size of the ruthenium-based alloy target blank.
[0019] (2) The present invention achieves coating of alloying element particles with ruthenium-based precursors through ball milling, crushing and coating processes without using the traditional powder metallurgy mixing process, thereby avoiding the problem of uneven mixing of pure ruthenium particles and alloying element particles, thereby achieving the purpose of reducing the cost and processing difficulty of ruthenium-based alloy targets.
[0020] (3) The present invention adopts a new composite powder preparation process combined with a hot pressing process, which can reduce the difficulty and cost of the preparation process of ruthenium-based alloy targets.
[0021] (4) The ruthenium-based alloy target material blank prepared by the process route of the present invention has the characteristics of controllable microstructure, high density and low oxygen content. At the same time, the equipment used in the preparation process of the present invention is highly versatile, which is conducive to subsequent industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The present invention is a process flow chart of the method for preparing a high-purity ruthenium-based alloy target. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following embodiments are merely simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0024] Example 1
[0025] The method for preparing the high-purity ruthenium-based alloy target of the present invention has the following process flow: Figure 1 As shown, the specific steps include:
[0026] (1) Ammonium chlororuthenate with a purity of 99.99% and spherical tungsten particles with a particle size of 10 μm are ball-milled using polytetrafluoroethylene and zirconium oxide ball milling balls to coat the ammonium chlororuthenate on the surface of the tungsten particles to obtain a composite powder; wherein the ball milling time is 6 hours, the ball milling speed is 300 r / min, and the ball milling process is a vacuum atmosphere; and the atomic content percentage of the tungsten particles in the composite powder is 10%, and the remainder is ruthenium.
[0027] (2) The composite powder obtained in step (1) is calcined and reduced in a tubular furnace; wherein the calcination temperature is 550°C, the time is 2 hours, and the calcination environment is vacuum; the reduction temperature is 500°C, the time is 3 hours, and the reducing atmosphere is an argon-hydrogen mixed atmosphere.
[0028] (3) vacuum hot pressing and sintering the composite powder treated in step (2) to obtain a ruthenium-based alloy target blank; wherein the sintering temperature is 1100° C., the holding time is 3 h, the welding pressure is 50 MPa, and the vacuum degree is less than 10 -3 Pa, heating rate 10℃ / min, after vacuum hot pressing sintering, finally a high-purity ruthenium-based alloy target blank is obtained; its density is 99.2%, and the average grain size is about 12μm.
[0029] Example 2
[0030] The method for preparing the high-purity ruthenium-based alloy target of the present invention has the following process flow: Figure 1 As shown, the specific steps include:
[0031] (1) Ammonium chlororuthenate with a purity of 99.99% and spherical tantalum particles with a particle size of 15 μm are ball-milled using polytetrafluoroethylene and zirconium oxide ball milling balls, so that the ammonium chlororuthenate is coated on the surface of the tantalum particles to obtain a composite powder; wherein the ball milling time is 12 h, the ball milling speed is 300 r / min, and the ball milling process is a vacuum atmosphere; and the atomic content percentage of the tantalum particles in the composite powder is 5%, and the remainder is ruthenium.
[0032] (2) The composite powder obtained in step (1) is calcined and reduced in a tubular furnace; wherein the calcination temperature is 650°C, the time is 3 hours, and the calcination environment is vacuum; the reduction temperature is 600°C, the time is 3 hours, and the reducing atmosphere is an argon-hydrogen mixed atmosphere.
[0033] (3) vacuum hot pressing and sintering the composite powder treated in step (2) to obtain a ruthenium-based alloy target blank; wherein the sintering temperature is 1200° C., the holding time is 4 h, the welding pressure is 70 MPa, and the vacuum degree is less than 10 -3 Pa, heating rate 10℃ / min, after vacuum hot pressing sintering, finally a high-purity ruthenium-based alloy target blank is obtained; its density is 99.3%, and the average grain size is about 20μm.
[0034] Example 3
[0035] The method for preparing the high-purity ruthenium-based alloy target of the present invention has the following process flow: Figure 1 As shown, the specific steps include:
[0036] (1) Ammonium chlororuthenate with a purity of 99.99% and spherical chromium particles with a particle size of 20 μm are ball-milled using polytetrafluoroethylene and zirconium oxide ball milling balls to coat the ammonium chlororuthenate on the surface of the chromium particles to obtain a composite powder; wherein the ball milling time is 12 h, the ball milling speed is 300 r / min, and the ball milling process is a vacuum atmosphere; and the atomic content percentage of the chromium particles in the composite powder is 25%, and the remainder is ruthenium.
[0037] (2) The composite powder obtained in step (1) is calcined and reduced in a tubular furnace; wherein the calcination temperature is 650°C, the time is 2 hours, and the calcination environment is vacuum; the reduction temperature is 600°C, the time is 6 hours, and the reducing atmosphere is an argon-hydrogen mixed atmosphere.
[0038] (3) vacuum hot pressing and sintering the composite powder treated in step (2) to obtain a ruthenium-based alloy target blank; wherein the sintering temperature is 1200° C., the holding time is 3 h, the welding pressure is 50 MPa, and the vacuum degree is less than 10 -3 Pa, heating rate 10℃ / min, after vacuum hot pressing sintering, finally obtain the blank of high-purity ruthenium-based alloy target; its density is 99.5%, and the average grain size is about 25μm.
[0039] Example 4
[0040] The method for preparing the high-purity ruthenium-based alloy target of the present invention has the following process flow: Figure 1 As shown, the specific steps include:
[0041] (1) Ammonium chlororuthenate with a purity of 99.99% and spherical tantalum particles with a particle size of 25 μm are ball-milled using polytetrafluoroethylene and zirconium oxide ball milling balls, so that the ammonium chlororuthenate is coated on the surface of the tantalum particles to obtain a composite powder; wherein the ball milling time is 12 h, the ball milling speed is 300 r / min, and the ball milling process is a vacuum atmosphere; and the atomic content percentage of the tantalum particles in the composite powder is 30%, and the remainder is ruthenium.
[0042] (2) The composite powder obtained in step (1) is calcined and reduced in a tubular furnace; wherein the calcination temperature is 550°C, the time is 5 hours, and the calcination environment is vacuum; the reduction temperature is 800°C, the time is 3 hours, and the reducing atmosphere is an argon-hydrogen mixed atmosphere.
[0043] (3) vacuum hot pressing and sintering the composite powder treated in step (2) to obtain a ruthenium-based alloy target blank; wherein the sintering temperature is 1300° C., the holding time is 6 h, the welding pressure is 70 MPa, and the vacuum degree is less than 10 -3Pa, heating rate 10℃ / min, after vacuum hot pressing sintering, finally a high-purity ruthenium-based alloy target blank is obtained; its density is 99.4%, and the average grain size is about 30μm.
[0044] The above-mentioned embodiments are only several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the scope of disclosure and protection of the present invention.
Claims
1. A method for preparing a high-purity ruthenium-based alloy target, characterized in that: The method specifically comprises the following steps: (1) ball milling ammonium chlororuthenate and spherical particles of alloying elements so that ammonium chlororuthenate is coated on the surface of the spherical particles of alloying elements to obtain composite powder; (2) calcining and reducing the composite powder obtained in step (1); (3) The composite powder treated in step (2) is subjected to vacuum hot pressing sintering to obtain a ruthenium-based alloy target.
2. The method for preparing a high-purity ruthenium-based alloy target according to claim 1, characterized in that: In step (1), polytetrafluoroethylene and zirconium oxide ball milling balls are used for ball milling.
3. The method for preparing a high-purity ruthenium-based alloy target according to claim 1, characterized in that: The purity of the ammonium chlororuthenate in step (1) is 99.99%.
4. The method for preparing a high-purity ruthenium-based alloy target according to claim 1, characterized in that: The spherical particles of alloying elements in step (1) are tantalum, chromium or tungsten.
5. The method for preparing a high-purity ruthenium-based alloy target according to claim 1, characterized in that: The particle size of the alloying element spherical particles in step (1) is 10 to 30 μm, and the purity is 99.99%.
6. The method for preparing a high-purity ruthenium-based alloy target according to claim 1, characterized in that: The atomic content percentage of the alloy element in the composite powder of step (1) is 1% to 30%, and the remainder is ruthenium element. The total atomic percentage of the alloy element and ruthenium element in the composite powder is 100%.
7. The method for preparing a high-purity ruthenium-based alloy target according to claim 1, characterized in that: The ball milling time in step (1) is 3 to 12 hours, the ball milling speed is 300 r / min, and the ball milling process is in a vacuum atmosphere.
8. The method for preparing a high-purity ruthenium-based alloy target according to claim 1, characterized in that: In step (2), the calcination temperature of the composite powder is 450-750° C., the time is 2-5 hours, and the calcination environment is vacuum; the reduction temperature is 500-800° C., the time is 3-6 hours, and the reduction atmosphere is an argon-hydrogen mixed atmosphere.
9. The method for preparing a high-purity ruthenium-based alloy target according to claim 1, characterized in that: During the vacuum hot pressing sintering in step (3), the sintering temperature is 1100-1300° C. and the insulation time is 3 h to 6 h.