Dissimilar metal brazing method

Through the low-temperature brazing method of different metals, stainless steel and aluminum alloys treated with nickel plating and tin burning are used for low-temperature welding, which solves the problems of complex vacuum brazing process and large thermal resistance, and achieves low-cost and efficient welding effects.

CN118875407APending Publication Date: 2024-11-01SHANGHAI GESI INFORMATION TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411188812.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, the vacuum brazing process is complex and the gas and liquid pipelines cannot be fully contacted with the radiator, resulting in large thermal resistance and it is difficult to achieve effective welding of stainless steel and aluminum alloys.

Method used

Using the method of low-temperature brazing of different metals, the metal tubes and aluminum alloys are subjected to nickel plating and tin hot treatment after grinding and ultrasonic cleaning, and using compression tooling constraints to replace the traditional fixing method, the tin brazing material is heated to low by heater. Welding is carried out at the temperature of the melting point of the tin brazing material.

Benefits of technology

It reduces operational difficulty and production costs, avoids thermal expansion mismatch and chemical reactions caused by high temperatures, improves the thermal conductivity and welding quality of welding, and simplifies equipment requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875407A_ABST
    Figure CN118875407A_ABST
Patent Text Reader

Abstract

The invention discloses a dissimilar metal brazing method which comprises the following steps: polishing a first to-be-welded part of a metal pipe and a second to-be-welded part of an aluminum alloy part, and ultrasonically cleaning the first to-be-welded part and the second to-be-welded part by acetone and alcohol in sequence; performing nickel plating and tin burning treatment on the first to-be-welded part and the second to-be-welded part respectively to form a first tin burning surface and a second tin burning surface; the first tinning face of the metal pipe and the second tinning face of the aluminum alloy part are spliced according to a preset assembling mode, and a pressing tool is used for pressing and restraining the metal pipe and the aluminum alloy part; and heating at least parts of the first tinning surface and the second tinning surface which are restrained by the pressing tool to a preset temperature by using a heater, and preserving heat for a preset heat preservation time. The method is low in cost and simple in technological process, the thermal conductivity is improved, and the problems that in the prior art, the vacuum brazing technological process is complex, and the thermal resistance is large due to the fact that vapor and liquid pipelines cannot make full contact with the radiator are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of brazing, and in particular to a low-temperature brazing method for dissimilar metals. Background Art

[0002] In the welding method for connecting the loop heat pipe radiator with the steam and liquid pipelines, the steam and liquid pipelines and the radiator need to be welded first. The steam and liquid pipelines are generally made of stainless steel, and the radiator is made of aluminum alloy plate. In the prior art, vacuum brazing is usually used to weld the steam and liquid pipelines and the radiator.

[0003] In the prior art, vacuum brazing is used to weld the steam and liquid pipelines to the radiator, but the cost is high and the process is complicated, which is not conducive to mass production. In addition, since the welding between the steam and liquid pipelines and the radiator is a dissimilar metal welding between stainless steel and aluminum alloy, and the steam and liquid pipelines are slender, this undoubtedly increases the difficulty of the welding operation. The use of clamps and rivets to fix the steam and liquid pipelines to the radiator will also make it impossible for the steam and liquid pipelines to fully contact the radiator, resulting in a large thermal resistance and reduced thermal conductivity, which makes it difficult to weld stainless steel and aluminum alloy together.

[0004] At present, no effective solution has been proposed for the problems in the prior art of complicated vacuum brazing process and large thermal resistance caused by insufficient contact between steam and liquid pipelines and radiators. Summary of the invention

[0005] In view of this, an embodiment of the present invention provides a method for low-temperature brazing of dissimilar metals to at least solve the problems in the prior art of complex vacuum brazing process and insufficient contact between steam and liquid pipelines and radiators resulting in high thermal resistance.

[0006] The embodiment of the present invention provides the following technical solutions:

[0007] An embodiment of the present invention provides a dissimilar metal brazing method, which is applied to welding between a metal tube and an aluminum alloy part. The method comprises:

[0008] Grinding the first to-be-welded portion of the metal tube and the second to-be-welded portion of the aluminum alloy part, and ultrasonically cleaning the first to-be-welded portion and the second to-be-welded portion using acetone and alcohol in sequence;

[0009] Performing nickel plating treatment on the first to-be-welded portion and the second to-be-welded portion respectively;

[0010] Performing tinning treatment on the first part to be welded and the second part to be welded after the nickel plating treatment respectively, so as to form a first tinning surface and a second tinning surface;

[0011] The first tinned surface of the metal tube and the second tinned surface of the aluminum alloy part are spliced ​​according to a predetermined assembly method, and the metal tube and the aluminum alloy part are compressed and constrained by using a compression tool, wherein the shape of the compression surface of the compression tool matches the shape of the compressed surface formed by the metal tube and the aluminum alloy part after being compressed and constrained;

[0012] Using a heater to heat at least a portion of the first tinning surface and the second tinning surface constrained by the pressing tool to a predetermined temperature, and keeping the temperature for a predetermined holding time, so that the tin solder on the first tinning surface and the second tinning surface is completely fused, wherein the predetermined temperature is greater than the melting point of the tin solder;

[0013] After stopping heating and cooling the first tinning surface and the second tinning surface to room temperature, the pressing tool is removed, and surface treatment is performed on the metal tube and the aluminum alloy part.

[0014] Furthermore, the metal tube is a stainless steel capillary tube.

[0015] Furthermore, the surface roughness of the first part to be welded and the second part to be welded are polished to be less than or equal to 2.0 μm, and the ultrasonic cleaning time using the acetone is 5 to 15 minutes, and the ultrasonic cleaning time using the alcohol is 5 minutes.

[0016] Furthermore, a pressing surface of the pressing tool is provided with a groove matching the metal tube, and the groove is used to press the surface of the metal tube that is not covered by the aluminum alloy part.

[0017] Furthermore, a heater is used to heat at least a portion of the constrained first tinning surface and the second tinning surface to 280° C. to 300° C. at a predetermined heating rate.

[0018] Furthermore, the predetermined insulation time is 10 to 40 minutes.

[0019] Furthermore, the predetermined heating rate is 5°C / min.

[0020] Furthermore, the step of stopping heating and cooling the first tinning surface and the second tinning surface to room temperature comprises:

[0021] Stop heating, and cool the first tinning surface and the second tinning surface to room temperature at a predetermined cooling rate.

[0022] Furthermore, the predetermined cooling rate is 10°C / min.

[0023] Furthermore, the surface treatment includes one or more of grinding, removing residues, and cleaning.

[0024] Compared with the prior art, the at least one technical solution adopted in the embodiment of the present invention can achieve the following beneficial effects:

[0025] The present invention discloses a dissimilar metal brazing method. After grinding and ultrasonic cleaning the welding part between the metal tube and the aluminum alloy part, the welding part is subjected to nickel plating and tinning treatment in sequence. Then, a pressing tool is used to compress and constrain the metal tube and the aluminum alloy part to replace the traditional fixing method of clamps and rivets, so that the metal tube and the aluminum alloy part can be better contacted, thereby solving the problem of insufficient contact between the steam and liquid pipelines and the radiator in the prior art, resulting in large thermal resistance.

[0026] Furthermore, a heater is used to heat the welding part of the metal tube and the aluminum alloy part. Since the melting point of the tin solder is low, the predetermined temperature of the heater is also low, thereby avoiding the problem of mismatch of thermal expansion coefficients caused by high temperature. At the same time, a lower temperature can also produce lower thermal stress and slow down or even inhibit chemical reactions.

[0027] Finally, compared with traditional vacuum brazing, the metal brazing method of the present invention has a lower process production cost, reduces the difficulty of operation, does not require the use of a vacuum brazing furnace, has simple equipment, and can perfectly solve the problems that need to be paid attention to in welding stainless steel and aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 A flow chart of a dissimilar metal brazing method according to an embodiment of the present invention;

[0030] Figure 2 A schematic diagram of a device for implementing a method for brazing dissimilar metals in an embodiment of the present invention;

[0031] Figure 3 Schematic diagram of the splicing of metal tubes and aluminum alloy parts in an embodiment of the present invention.

[0032] The accompanying drawings of the present invention are as follows:

[0033] 1. Pressing tool; 2. Metal pipe; 3. Aluminum alloy parts; 4. Heater. DETAILED DESCRIPTION

[0034] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0035] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0036] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0037] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0038] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the examples can be practiced without these specific details.

[0039] Steam and liquid pipelines are usually made of 316L stainless steel with an outer diameter of 3mm and an inner diameter of 2mm. The radiator uses an aluminum alloy plate. Due to the large difference in shape between the steam and liquid pipelines and the radiator, a special fixing method is required to fix the steam and liquid pipelines and the radiator during heating.

[0040] At present, vacuum brazing is used to weld steam and liquid pipelines to radiators. This method is not only costly but also has complicated process flow, such as the need to use a vacuum brazing furnace and maintain a vacuum environment during welding. Therefore, it is not conducive to mass production. The welding between steam and liquid pipelines and radiators belongs to the welding of dissimilar metals between 316L stainless steel and aluminum alloy, which requires many issues to be considered, such as the difference in thermal expansion between stainless steel and aluminum alloy under high temperature conditions, whether other chemical reactions will occur, etc. In addition, since the steam and liquid pipelines are slender, the difficulty of welding operation is increased during welding. When the steam and liquid pipelines and radiators are fixed by clamps and rivets, the steam and liquid pipelines cannot be fully contacted with the radiator, resulting in a large thermal resistance and reduced thermal conductivity, which makes it difficult for the brazing material to fully melt.

[0041] Moreover, since the steam and liquid pipelines are slender, with an outer diameter of only 3mm and an inner diameter of only 2mm, collapse or leakage after welding will cause throttling effect and flow loss, increasing the difficulty of welding operation. The use of clamps and rivets to fix the pipelines and radiators prevents sufficient contact between the metals, resulting in greater thermal resistance and reduced thermal conductivity.

[0042] Finally, since the temperature of vacuum brazing is generally between 600 and 1400°C, and the melting point of aluminum alloy is between 600 and 650°C, which is relatively low and not suitable for vacuum brazing, a low-temperature welding method is required to braze the aluminum alloy part 3.

[0043] Based on this, this specification embodiment proposes a processing solution: Figure 1 As shown, a dissimilar metal brazing method of the present invention is to perform nickel plating and tinning on the metal tube 2 and the aluminum alloy part 3 in sequence after grinding and cleaning the metal tube 2 and the aluminum alloy part 3, and use tin as the brazing brazing material, and then use the pressing tool 1 to compress and constrain the metal tube 2 and the aluminum alloy part 3, and finally use the heater 4 to heat the welding part between the metal tube 2 and the aluminum alloy part 3 to a predetermined temperature. The melting point of the tin brazing material of the present invention is much lower than the melting point of the aluminum alloy, and the melting point is relatively low. Therefore, after the metal tube 2 and the aluminum alloy are heated to the predetermined temperature, the aluminum alloy part 3 and the metal tube 2 will not chemically react, and the aluminum alloy and the metal tube 2 will not be mismatched due to different thermal expansion coefficients. Finally, the pressing tool 1 is used to compress and constrain the metal tube 2 and the aluminum alloy part 3, so that the welding part of the metal tube 2 and the aluminum alloy part 3 can be closely fitted, which solves the problem of complicated vacuum brazing process and large thermal resistance caused by insufficient contact between the steam and liquid pipelines and the radiator in the prior art.

[0044] The technical solutions provided by various embodiments of the present application are described below in conjunction with the accompanying drawings.

[0045] A dissimilar metal brazing method of the present invention is applied to the welding between a metal tube 2 and an aluminum alloy part 3. For example, it can be applied to the welding between a stainless steel metal tube 2 and an aluminum alloy part 3, the welding between an aluminum alloy tube and an aluminum alloy part 3, the welding between a copper tube and an aluminum alloy part 3, etc.

[0046] The aluminum alloy part 3 may be a plate-shaped structure, a groove-shaped structure, or the like.

[0047] The present invention takes the aluminum alloy part 3 as a radiator with a groove-shaped structure and the metal tube 2 as a 316L stainless steel tube as an example to describe in detail a dissimilar metal brazing method of the present invention.

[0048] like Figures 1 to 3 As shown, the dissimilar metal brazing method comprises:

[0049] Step S102: polish the first welding portion of the metal tube 2 and the second portion to be welded of the aluminum alloy part 3, and ultrasonically clean the first portion to be welded and the second portion to be welded using acetone and alcohol in sequence.

[0050] Among them, the first welding part of the metal tube 2 is the welding connection part between the metal tube 2 and the aluminum alloy part 3; the second welding part of the aluminum alloy part 3 is the welding connection part between the aluminum alloy part 3 and the metal tube 2.

[0051] Among them, the first welding part of the metal tube 2 and the second part to be welded of the aluminum alloy are polished so that the surface roughness of the first part to be welded and the second part to be welded are both less than or equal to 2.0 μm, so as to increase the contact area between the first part to be welded and the second part to be welded, and remove surface oxides or dirt to prepare for subsequent cleaning and welding.

[0052] When acetone is used to ultrasonically clean the first part to be welded and the second part to be welded, the cleaning time is 5 to 15 minutes, so as to preliminarily clean the first welding part and the second welding part and remove small surface particles, residual dirt and tiny metals generated during the grinding process.

[0053] Among them, when using alcohol to ultrasonically clean the first part to be welded and the second part to be welded, the cleaning time is 5 minutes, which is used to further clean the first part to be welded and the second part to be welded to ensure that the surface reaches a high degree of cleanliness and reduce the impact of impurities on the performance of the welding part.

[0054] For example, when the metal tube 2 is a stainless steel metal tube 2 and the aluminum alloy part 3 is a radiator with a groove-shaped structure, the outer surface to be welded of the metal tube 2 and the groove to be welded portion of the aluminum alloy part 3 are polished and ultrasonically cleaned in sequence.

[0055] Step S102 can optimize the surface state of the first welding part and the second welding part before welding, improve the welding quality, and ensure the firmness and durability of the weld by performing surface treatment on the first welding part and the second welding part.

[0056] Step S104, performing nickel plating treatment on the first part to be welded and the second part to be welded respectively.

[0057] Among them, by nickel plating the first part to be welded and the second part to be welded, a good intermediate layer can be formed between the first part to be welded and the second part to be welded, so as to improve the operability and joint strength of metal welding, which is particularly important for metals such as stainless steel and aluminum alloy that are difficult to weld directly.

[0058] The first part to be welded and the second part to be welded are respectively subjected to nickel plating, which can also increase the hardness of the surface and promote uniform heat conduction, so as to facilitate the transfer of heat after subsequent heating by the heater 4.

[0059] For example, when the metal tube 2 is a stainless steel metal tube 2 and the aluminum alloy part 3 is a radiator, the outer surface to be welded of the metal tube 2 and the groove to be welded of the aluminum alloy part 3 are respectively subjected to nickel plating treatment.

[0060] In step S104, the first part to be welded and the second part to be welded are respectively subjected to nickel plating, thereby improving the performance of the material itself, and achieving the purpose of protecting the substrate, preventing corrosion, improving hardness and wear resistance, improving chemical stability and improving welding performance.

[0061] Step S106, performing tinning treatment on the first part to be welded and the second part to be welded after the nickel plating treatment, respectively, to form a first tinning surface and a second tinning surface.

[0062] Among them, since the melting point of the aluminum alloy part 3 is relatively low and the melting point of the tin solder is between 227 and 232°C, the tin solder can be used as the temperature requirement of the dissimilar metal brazing method of the present invention, while the melting points of other solders are much higher than that of the tin solder and do not meet the temperature requirements of the low-temperature brazing of the present invention.

[0063] When the metal tube 2 is a stainless steel metal tube 2 and the aluminum alloy part 3 is a radiator, the outer surface to be welded of the metal tube 2 and the groove to be welded of the aluminum alloy part 3 are tinned respectively.

[0064] Step S106 performs tinning on the first part to be welded and the second part to be welded, which can better wet the nickel plating layer and improve the fluidity of the tin solder on the metal surface to ensure a more uniform and stronger welding joint; and the tinning treatment can fill the tiny unevenness and gaps on the surface of the first part to be welded and the second part to be welded, reducing common defects such as voids and cracks in the welding process.

[0065] Step S108, splice the first tinned surface of the metal tube 2 and the second tinned surface of the aluminum alloy part 3 according to a predetermined assembly method, and use a pressing tool 1 to compress and constrain the metal tube 2 and the aluminum alloy part 3, wherein the shape of the pressing surface of the pressing tool 1 matches the shape of the pressed surface formed by the metal tube 2 and the aluminum alloy part 3 after being pressed and constrained.

[0066] Among them, before welding the metal tube 2 and the aluminum alloy part 3, it is necessary to use a pressing tool 1 to compress and constrain the already spliced ​​metal tube 2 and the aluminum alloy part 3 to avoid displacement between the metal tube 2 and the aluminum alloy part 3 during the heating process, which will cause the metal tube 2 and the aluminum alloy part 3 to be unable to be welded according to the predetermined assembly method.

[0067] Among them, by setting the shape of the pressing surface of the pressing tool 1 to match the shape of the pressed surface formed by the metal tube 2 and the aluminum alloy part 3 after being pressed and constrained, the metal tube 2 and the aluminum alloy part 3 can be better pressed and constrained to ensure uniform and stable pressing.

[0068] Specifically, the pressing surface of the pressing tool 1 is provided with a groove matching the metal tube 2, and the groove is used to press the surface of the metal tube 2 not covered by the aluminum alloy part 3, so that the pressing surface of the pressing tool 1 can apply uniform and stable pressure to at least the first part of the metal tube 2 to be welded.

[0069] Among them, pressing the metal tube 2 and the aluminum alloy part 3 by the pressing tool 1 can also maintain close contact between the metal tube 2 and the aluminum alloy part 3 to prevent misalignment, ensure the accuracy and consistency of the joint, and also help improve the flow and wetting effect of the tin solder to ensure the welding quality.

[0070] For example, when the metal tube 2 is a stainless steel metal tube 2 and the aluminum alloy part 3 is a radiator, the outer surface of the metal tube 2 to be welded is placed inside the groove to be welded portion of the aluminum alloy part 3, a portion of the surface of the metal tube 2 is embedded in the groove to be welded portion of the aluminum alloy part 3, and the other half is exposed to the outside and compressed by the compression tool 1, so that the outer surface of the metal tube 2 to be welded and the groove to be welded portion can be tightly connected, so that the metal tube 2 and the aluminum alloy part 3 can be fully in contact, thereby increasing the heat exchange area and improving the thermal conductivity.

[0071] Step S108 performs stable compression on the aluminum alloy part 3 and the metal tube 2 by means of the compression tool 1, so that a uniform contact interface is formed between the first part to be welded and the second part to be welded, the filling and bonding performance of the tin solder is improved, and the metal tube 2 and the aluminum alloy part 3 are ensured to maintain an ideal geometric position and contact shape during the bonding process, so as to obtain a high-quality and reliable connection effect.

[0072] Step S110, using the heater 4 to slowly heat at least a portion of the first tinned surface and the second tinned surface constrained by the compression tool 1 to a predetermined temperature, and keep the temperature for a predetermined holding time so that the tin solder on the first tinned surface and the second tinned surface is completely fused, wherein the predetermined temperature is greater than the melting point of the tin solder.

[0073] The heater 4 can be used to heat the first tinning surface and the second tinning surface partially, so the operation is more flexible and there is no need to worry about the problem of the metal tube 2 and the aluminum alloy part 3 being too large in size.

[0074] Among them, after the metal tube 2 and the aluminum alloy part 3 are fixed and constrained, the heater 4 is used to heat the welding part of the metal tube 2 and the aluminum alloy part 3, so that at least part of the first tinned surface and the second tinned surface are slowly heated to a predetermined temperature, and after being heated to the predetermined temperature, they are kept warm for a predetermined holding time, so that the tin solder on the first tinned surface and the second tinned surface is completely fused.

[0075] The melting point of the tin solder is between 227 and 232° C., so when the heater 4 is used for heating, it is only necessary to heat the predetermined temperature to greater than 232° C. to completely melt the tin solder and complete the welding of the metal tube 2 and the aluminum alloy part 3 .

[0076] For the metal tube 2 and the aluminum alloy part 3, since the melting point of the aluminum alloy part 3 is relatively high, the temperature is slightly greater than 232°C. It belongs to low-temperature welding for both the aluminum alloy part 3 and the stainless steel tube, thereby reducing the thermal influence and better dealing with the problem of mismatch in thermal expansion coefficients. The lower temperature can not only produce lower thermal stress, but also slow down or even inhibit chemical reactions.

[0077] Furthermore, the heater 4 may be used to heat at least a portion of the constrained first tinning surface and the second tinning surface to 280-300° C. at a predetermined heating rate.

[0078] The predetermined heating rate may be 5° C. / min, and the predetermined heat preservation time may be 10 to 40 min.

[0079] Wherein, by heating the space between the first tinning surface and the second tinning surface at a predetermined heating rate, preheating of the first tinning surface and the second tinning surface can be achieved during the heating process.

[0080] Step S110 can effectively prevent the occurrence of cold cracks, hot cracks and hardened structures in the heat-affected zone by heating at a predetermined heating rate and keeping the temperature for a predetermined holding time. It also avoids the shrinkage stress in the end area caused by rapid cooling and heating during welding of the welding joint, thereby causing cracks. Preheating can reduce shrinkage stress and prevent the occurrence of cracks. In addition, preheating can remove residual oil, moisture and other factors that affect the quality of the weld, and can also promote the overflow of hydrogen in the weld to prevent defects such as pores or cracks.

[0081] Step S112, stop heating, and after the first tinning surface and the second tinning surface are cooled to room temperature, remove the pressing tool 1, and perform surface treatment on the metal tube 2 and the aluminum alloy part 3.

[0082] After the preheating and holding time, the heating is stopped to allow the first tinned surface and the second tinned surface to cool to room temperature. At this time, the welding is completed, the pressing tool 1 can be removed, and the metal tube 2 and the aluminum alloy are surface treated.

[0083] Further, step S112 includes:

[0084] Step S112a, stop heating, and cool the first tinning surface and the second tinning surface to room temperature at a predetermined cooling rate.

[0085] The predetermined cooling rate is 10°C / min.

[0086] By cooling at a predetermined cooling rate, it is also possible to avoid the problem of shrinkage stress in the end area caused by extremely rapid cooling, thereby causing cracks.

[0087] The surface treatment of the metal tube 2 and the aluminum alloy includes processes such as grinding, removing residues and cleaning.

[0088] The heating and cooling process of the present invention is as follows: when heating the metal tube 2 and the aluminum alloy part 3 that have been fixed and constrained, the pressure is tested with a pressing tool 1 to avoid dislocation of the metal tube 2 and the aluminum alloy; the temperature is raised to 280-300°C at a rate of 5°C / min, and preheated and kept warm for 10 minutes, and the condition of the workpiece is observed during the whole process, so that the brazing insulation time is controlled at 10-40 minutes, and the heating is stopped after the tin solder is completely melted and fused, and the temperature is lowered at a rate of 10°C / min until it cools to room temperature.

[0089] Compared with vacuum brazing in the prior art, the present invention adopts low-temperature brazing, which not only meets the working temperature lower than the melting point of dissimilar metals, but also has simple equipment and convenient operation, thereby reducing production and processing costs, thereby being able to more efficiently solve the problem of welding connection between the loop heat pipe radiator and the steam and liquid pipelines.

[0090] The present invention discloses a dissimilar metal brazing method, which uses low-temperature welding and requires a temperature of only 280 to 300°C, which is far lower than the melting points of stainless steel and aluminum alloy. The method of preheating and heat preservation is adopted to reduce the thermal influence and better deal with the problem of mismatch in thermal expansion coefficients. The lower temperature can not only produce lower thermal stress, but also slow down or even inhibit chemical reactions.

[0091] The dissimilar metal brazing method of the present invention does not need to use vacuum brazing, reduces process production costs, reduces operation difficulty, does not need to use a vacuum brazing furnace, uses simple equipment, and can perfectly solve the problems that need to be paid attention to in welding 316L stainless steel and aluminum alloy. A specific tool is used to fix the welded parts so that the pipeline and the radiator can fully contact, increase the heat exchange area, and improve thermal conductivity. In summary, the prior art is significantly superior to the vacuum brazing technology of the prior art.

[0092] The present invention will be further described below in conjunction with specific embodiments.

[0093] The inventors of the present invention have implemented a test in the following embodiments: the batch of test pieces has a total of 300 pieces, and the test pieces respectively use stainless steel capillaries and aluminum alloy plate radiators of different sizes. Among them, the test pieces of 100 stainless steel capillaries have the following dimensions: outer diameter 3mm, inner diameter 2mm, and unfolded length 1000mm; the test pieces of 100 stainless steel capillaries have the following dimensions: outer diameter 5mm, inner diameter 4mm, and unfolded length 1500mm; the test pieces of the remaining 100 stainless steel capillaries have the following dimensions: outer diameter 3mm, inner diameter 2mm, and unfolded length 2000mm. The radiators all use aluminum alloy plates of 300mm×50mm×20mm. The surfaces to be welded of the 316L stainless steel capillary and the aluminum alloy plate radiator are polished and cleaned for 10-20 minutes, the groove surface to be welded where the aluminum alloy plate radiator is connected to the 316L stainless steel capillary and the surface to be welded of the stainless steel capillary are plated with bright nickel, and then the surface of the nickel-plated layer and the surface of the stainless steel tube are hot-tinned, and then a specific tool is used to fix and constrain the connection between the groove of the aluminum alloy plate radiator and the 316L stainless steel capillary, so that the pipe is placed in the plate groove, and finally a specific heater 4 is used to heat and pressurize the constrained surface to be welded, and then it is cooled to room temperature and surface treated.

[0094] The specimens were subjected to thermodynamic tests and tensile performance tests, and the test results were all correct. All 300 specimens were successfully completed, meeting the work requirements, and were simple to operate and low-cost.

[0095] In this specification, the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the product embodiment described later, since it corresponds to the method, the description is relatively simple, and the relevant parts can be referred to the partial description of the system embodiment.

[0096] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A method for brazing dissimilar metals, It is characterized in that Applied to welding between a metal pipe and an aluminum alloy part, the method comprises: Grinding the first to-be-welded portion of the metal tube and the second to-be-welded portion of the aluminum alloy part, and ultrasonically cleaning the first to-be-welded portion and the second to-be-welded portion using acetone and alcohol in sequence; Performing nickel plating treatment on the first to-be-welded portion and the second to-be-welded portion respectively; Performing tinning treatment on the first part to be welded and the second part to be welded after the nickel plating treatment respectively, so as to form a first tinning surface and a second tinning surface; The first tinned surface of the metal tube and the second tinned surface of the aluminum alloy part are spliced ​​according to a predetermined assembly method, and the metal tube and the aluminum alloy part are compressed and constrained by using a compression tool, wherein the shape of the compression surface of the compression tool matches the shape of the compressed surface formed by the metal tube and the aluminum alloy part after being compressed and constrained; Using a heater to heat at least a portion of the first tinning surface and the second tinning surface constrained by the pressing tool to a predetermined temperature, and keeping the temperature for a predetermined holding time, so that the tin solder on the first tinning surface and the second tinning surface is completely fused, wherein the predetermined temperature is greater than the melting point of the tin solder; After stopping heating and cooling the first tinning surface and the second tinning surface to room temperature, the pressing tool is removed, and surface treatment is performed on the metal tube and the aluminum alloy part.

2. The dissimilar metal brazing method according to claim 1, It is characterized in that The metal tube is a stainless steel capillary tube.

3. The dissimilar metal brazing method according to claim 1, It is characterized in that The surface roughness of the first part to be welded and the second part to be welded are both polished to less than or equal to 2.0 μm, and the ultrasonic cleaning time using the acetone is 5 to 15 minutes, and the ultrasonic cleaning time using the alcohol is 5 minutes.

4. The dissimilar metal brazing method according to claim 3, It is characterized in that A groove matching the metal tube is provided on the pressing surface of the pressing tool, and the groove is used to press the surface of the metal tube that is not covered by the aluminum alloy part.

5. The dissimilar metal brazing method according to claim 4, It is characterized in that A heater is used to heat at least a portion of the constrained first tinning surface and the second tinning surface to 280° C. to 300° C. at a predetermined heating rate.

6. The dissimilar metal brazing method according to claim 5, It is characterized in that The predetermined insulation time is 10 to 40 minutes.

7. The dissimilar metal brazing method according to claim 5, It is characterized in that The predetermined heating rate is 5°C / min.

8. The dissimilar metal brazing method according to any one of claims 5 to 7, It is characterized in that The step of stopping heating and cooling the first tinning surface and the second tinning surface to room temperature comprises: Stop heating, and cool the first tinning surface and the second tinning surface to room temperature at a predetermined cooling rate.

9. The dissimilar metal brazing method according to claim 8, It is characterized in that The predetermined cooling rate is 10°C / min.

10. The dissimilar metal brazing method according to claim 1, It is characterized in that The surface treatment includes one or more of grinding, removing residues, and cleaning.

Citation Information

Patent Citations

  • Method for large-area low-defect rate soldering of dissimilar metallic combination drive pipe structure

    CN103624356A

  • Loop heat pipe evaporator large-area soldering method

    CN103639559A

  • Stainless steel / aluminum alloy special metal brazing assembly-connecting method

    CN109759663A

  • Brazing method between aluminum-based metal and different metal

    JP2004066324A