Resistance spot welding method for high-strength aluminum alloy plate
By using a fixed inverter spot welding machine in aluminum alloy plate resistance spot welding, gradually adjusting the welding current and pressure, combining appearance and metallographic detection, optimizing welding parameters, the splashing and splashing problems are solved, and the welding quality and operability are improved , meets the welding needs of high-strength aluminum alloy plates.
Patent Information
- Application Number
- CN202411234637.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-01
AI Technical Summary
Resistance spot welding of high-strength aluminum alloy plates is prone to splashing and splashing, resulting in poor welding quality, and the adhesion between the electrode and the workpiece seriously affects the subsequent welding efficiency and quality.
Determine the welding range of aluminum alloy samples through peeling experiments, and use a fixed inverter spot welding machine to gradually increase the spot welding sample preparation within a certain welding current range. Combined with appearance inspection and internal metallographic inspection, the welding parameters are screened and optimized to improve welding quality.
It realizes the reliable welding quality of high-strength aluminum alloy plate joints, enhances the operability and promotion value of welding, and can select appropriate welding parameters according to user strength requirements.
Smart Images

Figure CN118875449A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy plate joint connection, and in particular relates to a high-strength aluminum alloy plate resistance spot welding method. Background Art
[0002] Compared with other metal materials such as steel, aluminum alloy has a lower density, lighter weight, and corrosion resistance. It has significant advantages in lightweight equipment manufacturing and is the preferred solution for energy conservation and emission reduction in the automotive industry. 6056 aluminum alloy is a high-strength aluminum alloy material with high strength and good plasticity. It is widely used in aerospace, automobile manufacturing and other fields. In the aerospace field, this aluminum alloy is often used to manufacture aircraft structural parts and engine parts. The high strength and light weight characteristics make the aircraft more energy-saving and environmentally friendly; in the automotive manufacturing field, it is often used to manufacture body and chassis parts, which can reduce the weight of the vehicle and improve fuel efficiency. Aluminum alloy materials are connected in a suitable way to form a structure with a certain strength, thereby realizing the function of the equipment. Among them, resistance spot welding is a widely used connection form. The welded workpiece is pressed between two electrodes, and the resistance heat effect generated by the current flowing through the joint through the contact surface of the workpiece and the nearby area is used to heat the workpiece to a molten state, so that the workpieces in contact with each other are fused together. However, due to the low resistance of the aluminum alloy plate, the current required for spot welding is large, which is very easy to produce ablation and spatter, affecting the welding quality. Therefore, studying the resistance spot welding process of high-strength aluminum alloy plates, finding out the factors affecting welding quality, and determining the reasonable welding area are of practical significance for improving the comprehensive performance of high-strength aluminum alloy plates, improving welding efficiency, promoting the high-strength and lightweight development of automobile structures, and achieving energy conservation and emission reduction goals.
[0003] High-strength aluminum alloy resistance spot welding is prone to spattering and splattering. On the one hand, aluminum is very active, and it is very easy to form an oxide film on the surface of aluminum alloy materials. This oxide film has a dense structure, a very high melting point, and extremely poor electrical conductivity. This makes the contact resistance on the contact surface relatively large, and under hard standard welding conditions, more heat is generated on the contact surface. On the other hand, aluminum alloy materials have a low melting point and a narrow plastic temperature range when heated and melted, which can easily cause spattering on the contact surface between the workpieces and adhesion between the electrode and the workpiece. Once this happens, it will take away some heat and molten metal, seriously affecting the size of the molten core diameter, which is extremely unfavorable to the quality of the weld. At the same time, the adhesion and spattering between the electrode and the workpiece seriously destroy the continuity of the electrode surface, thereby worsening the contact state between the electrode and the workpiece during subsequent welding of the weld, thereby aggravating the generation of spatter, local melting and adhesion, which is even more unfavorable to the surface quality of the weld. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a method for resistance spot welding of high-strength aluminum alloy plates.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A high-strength aluminum alloy plate resistance spot welding method comprises the following steps:
[0007] S1 Determine the weldable range of aluminum alloy samples through peeling test;
[0008] S2: When the welding time and welding pressure are constant, the welding current is increased by equal amounts in each group within the interval to prepare the spot welding sample;
[0009] S3 ensures that the welding time in step S2 remains unchanged, changes the welding pressure and repeats step S2;
[0010] S4 performs a stripping test on the qualified samples, and records the nugget diameter and welding current data after the joint is stripped;
[0011] S5 performs a tensile strength test on the sample, and compares the diameter of the sample nugget with the data in step S4, and screens out data that do not meet the requirements;
[0012] S6: According to the experimental record data of step S5, a weldable area map of the aluminum alloy material is prepared.
[0013] Preferably, in step S1, the aluminum alloy sample is an aluminum alloy plate with a thickness less than 3 mm.
[0014] Preferably, in step S2, welding is performed on a fixed inverter spot welding machine, and the welding parameters are:
[0015] Welding pressure 2500N~8000N; welding current 15~42kA; welding time 120~450mms; single pulse welding.
[0016] Preferably, the electrode cap of the fixed inverter spot welding machine has a diameter of 16 to 25 mm, a spherical end with a spherical radius of 20 to 125 mm, a surface roughness less than 3.2 μm, and is made of CrCu with a hollow interior to facilitate the flow of welding cooling water.
[0017] Preferably, in step S2, the welding current is increased in increments within a range of 0.5 to 1 kA.
[0018] Preferably, the step S3 further includes:
[0019] Observe the appearance quality of the sample;
[0020] Use metallographic method to detect the internal quality of the weld core of the sample and check whether there are shrinkage holes, cracks, and unfused defects;
[0021] The welding current at which spatter is generated is recorded.
[0022] Preferably, in step S6, the weldable area diagram of the aluminum alloy material is used to display the welding pressure corresponding to the aluminum alloy material within its welding current.
[0023] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0024] In the present invention, a fixed inverter spot welding machine is used to make welding samples. Within a certain welding current range, spot welding samples are prepared in increments of each group. The welding quality is evaluated by appearance inspection and internal metallographic inspection. According to the selected welding process (welding current range), the sample shearing and cross tensile mechanical property tests are carried out, and the process parameters are optimized by comprehensive analysis. The high-strength aluminum alloy plate joint welded by this welding process can select corresponding welding parameters within the weldable area according to the user's strength requirements. The welding quality is reliable, the operability is strong, and it has good promotion value. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a spot welding area diagram of the high-strength aluminum alloy material of the present invention;
[0026] Figure 2 It is a metallographic detection diagram of the weld nugget of the aluminum alloy material in the embodiment of the present invention. DETAILED DESCRIPTION
[0027] The specific embodiments of the present invention are described in detail below.
[0028] The "range" disclosed in the present invention is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 10 to 50 is listed for a specific parameter, it is understood that the range of 10 to 40 and 20 to 50 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In this application, unless otherwise specified, the range of values "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the range of values "0 to 5" means that all real numbers between "0 to 5" have been fully listed in this article, and "0 to 5" is only an abbreviation of these numerical combinations.
[0029] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0030] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0031] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0032] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0033] Unless otherwise specified, the reaction is carried out at room temperature and pressure.
[0034] Unless otherwise specified, all parts or percentages are by weight.
[0035] In the present invention, all substances used are known substances and can be purchased or synthesized by known methods.
[0036] In the present invention, the devices or equipment used are all conventional devices or equipment known in the art and are commercially available.
[0037] The specific implementation of the high-strength aluminum alloy plate resistance spot welding method of the present invention is further described below in conjunction with the embodiments. The high-strength aluminum alloy plate resistance spot welding method of the present invention is not limited to the description of the following embodiments.
[0038] Embodiment 1:
[0039] A high-strength aluminum alloy plate resistance spot welding method comprises the following steps:
[0040] S1 Figure 2 As shown in the figure, the weldable range of aluminum alloy samples is determined through peeling test;
[0041] S2: When the welding time and welding pressure are constant, the welding current is increased by equal amounts in each group within the interval to prepare the spot welding sample;
[0042] S3 ensures that the welding time in step S2 remains unchanged, changes the welding pressure and repeats step S2;
[0043] S4 performs a stripping test on the qualified samples, and records the nugget diameter and welding current data after the joint is stripped;
[0044] S5 performs a tensile strength test on the sample, and compares the diameter of the sample nugget with the data in step S4, and screens out data that do not meet the requirements;
[0045] S6: According to the experimental record data of step S5, a weldable area map of the aluminum alloy material is prepared.
[0046] Furthermore, in step S1, the aluminum alloy sample is an aluminum alloy plate with a thickness less than 3 mm.
[0047] Further, in step S2, welding is performed on a fixed inverter spot welding machine, and the welding parameters are:
[0048] Welding pressure 2500N; welding current 15kA; welding time 120mms; single pulse welding.
[0049] Furthermore, the electrode cap of the fixed inverter spot welding machine has a diameter of 16 mm, a spherical end, a spherical radius of 20 mm, a surface roughness of less than 3.2 μm, a material of CrCu, and a hollow interior to facilitate the flow of welding cooling water.
[0050] Furthermore, in step S2, the welding current is increased by 0.5 kA within the interval.
[0051] Furthermore, step S3 further includes:
[0052] Observe the appearance quality of the sample;
[0053] Use metallographic method to detect the internal quality of the weld core of the sample and check whether there are shrinkage holes, cracks, and unfused defects;
[0054] The welding current at which spatter is generated is recorded.
[0055] Further, such as Figure 1 As shown, in step S6, the aluminum alloy material weldable area diagram is used to display the welding pressure corresponding to the aluminum alloy material within its welding current.
[0056] Embodiment 2:
[0057] A high-strength aluminum alloy plate resistance spot welding method, the other steps are similar to those of Example 1, further, in step S2, the welding is performed on a fixed inverter spot welding machine, and the welding parameters are:
[0058] Welding pressure 5000N; welding current 28kA; welding time 280mms; single pulse welding.
[0059] Furthermore, the electrode cap of the fixed inverter spot welding machine has a diameter of 20 mm, a spherical end, a spherical radius of 70 mm, a surface roughness of less than 3.2 μm, a material of CrCu, and a hollow interior to facilitate the flow of welding cooling water.
[0060] Furthermore, in step S2, the welding current is increased by 0.8 kA within the interval.
[0061] Embodiment 3:
[0062] A high-strength aluminum alloy plate resistance spot welding method, the other steps are similar to those of Example 1, further, in step S2, the welding is performed on a fixed inverter spot welding machine, and the welding parameters are:
[0063] Welding pressure 8000N; welding current 42kA; welding time 450mms; single pulse welding.
[0064] Furthermore, the electrode cap of the fixed inverter spot welding machine has a diameter of 25 mm, a spherical end, a spherical radius of 125 mm, a surface roughness of less than 3.2 μm, and is made of CrCu with a hollow interior to facilitate the flow of welding cooling water.
[0065] Furthermore, in step S2, the welding current is increased in increments of 1 kA within the interval.
[0066] Embodiment 4:
[0067] A high-strength aluminum alloy plate resistance spot welding method, the implementation process of which includes:
[0068] Equipment requirements: Fixed inverter spot welding machine, welding machine electrode cap diameter 16mm, end spherical, spherical radius 20mm, surface roughness (Rp) less than 3.2μm. Made of CrCu, hollow inside to facilitate the flow of welding cooling water.
[0069] Process parameter settings: welding time 300ms, pressure 4000N, welding current from 27kA to 31kA. The test results of the samples after welding are shown in the table below.
[0070]
[0071] As can be seen from the table above, when the user requires the spot welding strength of the aluminum alloy plate to reach more than 6000N, the welding process can be selected as follows: welding time 300ms, pressure 4000N, welding current between 28kA and 30kA, see Figure 1 Center (C, F) point.
[0072] Embodiment 5:
[0073] A high-strength aluminum alloy plate resistance spot welding method, the implementation process of which includes:
[0074] Equipment requirements: Fixed inverter spot welding machine, welding machine electrode cap diameter 16mm, end spherical, spherical radius 20mm, surface roughness (Rp) less than 3.2μm. Made of CrCu, hollow inside to facilitate the flow of welding cooling water.
[0075] Process parameter settings: welding time 300ms, pressure 6000N, welding current from 29kA to 36kA. The test results of the samples after welding are shown in the table below.
[0076]
[0077] As can be seen from the table above, when the user requires the spot welding strength of the aluminum alloy plate to reach more than 7000N, the welding process can be selected as follows: welding time 300ms, pressure 6000N, welding current between 30kA and 35kA, see Figure 1 (B, E) points.
[0078] Embodiment 6:
[0079] A high-strength aluminum alloy plate resistance spot welding method, the implementation process of which includes:
[0080] Equipment requirements: Fixed inverter spot welding machine, welding machine electrode cap diameter 16mm, end spherical, spherical radius 20mm, surface roughness (Rp) less than 3.2μm. Made of CrCu, hollow inside to facilitate the flow of welding cooling water.
[0081] Process parameter settings: welding time 300ms, pressure 8000N, welding current from 36kA to 41kA. The test results of the samples after welding are shown in the table below.
[0082]
[0083] From the table above, we can see that when the user requires the spot welding strength of aluminum alloy plate to reach more than 8000N, the matching welding process can be selected as follows: welding time 300ms, pressure 8000N, welding current between 37kA and 41kA, see Figure 1 (A, D) points.
[0084] In summary, this application uses a fixed inverter spot welding machine to make welding samples. Within a certain welding current range, spot welding samples are prepared in increments of each group; welding quality is evaluated by appearance inspection and internal metallographic inspection; according to the selected welding process (welding current range), the sample shearing and cross tensile mechanical properties tests are carried out, and the process parameters are optimized by comprehensive analysis. The high-strength aluminum alloy plate joints welded by this welding process can select corresponding welding parameters within the weldable area according to the user's strength requirements. The welding quality is reliable, the operability is strong, and it has good promotion value.
[0085] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for resistance spot welding of high-strength aluminum alloy plates, characterized in that: The following steps are involved: S1 determines the weldability range of aluminum alloy specimens through peeling test; S2: When welding time and welding pressure are constant, the welding current is increased by equal amounts in each group within the interval to prepare spot welding samples; S3 ensures that the welding time in step S2 remains unchanged, changes the welding pressure and repeats step S2; S4 performs a stripping test on the qualified samples and records the nugget diameter and welding current data after the joint is stripped; S5 performs a tensile strength test on the sample, and compares the sample nugget diameter with the data in step S4 to filter out data that does not meet the requirements; S6: Create a weldable area map of the aluminum alloy material based on the experimental record data of step S5.
2. The method for resistance spot welding of a high-strength aluminum alloy plate according to claim 1, wherein: In step S1, the aluminum alloy sample is an aluminum alloy plate with a thickness of less than 3 mm.
3. The method for resistance spot welding of a high-strength aluminum alloy plate according to claim 1, wherein: In step S2, welding is performed on a fixed inverter spot welder, and the welding parameters are: Welding pressure 2500N~8000N; welding current 15~42kA; welding time 120~450mms; single pulse welding.
4. A method for resistance spot welding of high-strength aluminum alloy plates according to claim 3, characterized in that: The electrode cap of the fixed inverter spot welder has a diameter of 16 to 25 mm, a spherical end with a spherical radius of 20 to 125 mm, a surface roughness less than 3.2 μm, is made of CrCu, and is hollow inside to facilitate the flow of welding cooling water.
5. The method for resistance spot welding of a high-strength aluminum alloy plate according to claim 1, wherein: In step S2, the welding current is increased in increments within a range of 0.5 to 1 kA.
6. The method for resistance spot welding of a high-strength aluminum alloy plate according to claim 1, wherein: The step S3 further includes: Observe the appearance quality of the sample; Use metallographic method to test the internal quality of the weld core of the sample to check whether there are shrinkage holes, cracks, and lack of fusion defects; Record the welding current when spatter occurs.
7. The method for resistance spot welding of a high-strength aluminum alloy plate according to claim 1, wherein: In step S6, the aluminum alloy material weldable area diagram is used to display the corresponding welding pressure of the aluminum alloy material within its welding current.