Modified ammonia-soluble quaternary ammonium copper, anti-corrosion oriented strand board, preparation method and application
Through the preparation of modified ammonia-soluble quaternary ammonium copper and uniform distribution in directional particle board, the problem of large amount of preservatives in the prior art is solved, and a more efficient and environmentally friendly anticorrosion effect is achieved, and it is suitable for the anticorrosion treatment of wood and bamboo.
Patent Information
- Application Number
- CN202410905835.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-08
AI Technical Summary
When existing ammonia-soluble quaternary ammonium copper is used for wood anti-corrosion, the anti-corrosion effect increases with the increase of adhesive usage, but it leads to large adhesive usage, which is not environmentally friendly, and it is difficult to penetrate evenly during the production process of directional particleboard, affecting the anti-corrosion effect.
By using the preparation method of modified ammonia-soluble quaternary ammonium copper, by mixing poly(styrene-butyl acrylate-acrylic acid)/silica nanocomposite emulsion with ammonia-soluble quaternary ammonium copper, and using phenolic resin adhesive as the carrier, The surface and core layers of directional particle board are evenly distributed to improve corrosion resistance.
The anticorrosion performance is significantly enhanced with less adhesive usage, the anticorrosion effect of directional particleboard is improved, adapted to the existing production process, and is more environmentally friendly and safe, reaching a strong corrosion resistance level.
Smart Images

Figure CN118876183A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corrosion materials and functional artificial boards, and in particular relates to modified ammonia-soluble quaternary ammonium copper and anti-corrosion oriented strand board, a preparation method and application thereof. Background Art
[0002] Oriented strand board has excellent mechanical properties and is one of the man-made board products for structure. With the development of the wood building structure industry, oriented strand board is increasingly used as roof panels, floor panels and wall panels of wooden structure buildings. Oriented strand board without anti-corrosion treatment is susceptible to mold and decay fungi. Under certain conditions, it decays in a similar way to solid wood. The destructive effect of early decay on the board will cause the building structure to lose most of its mechanical strength and anti-deformation ability. Therefore, it is of great significance to treat the oriented strand board with anti-corrosion to improve its anti-corrosion performance for the safe use of buildings.
[0003] The commonly used preservatives in the market mainly include two water-soluble preservatives, copper chromium arsenic and ammonia soluble quaternary ammonium copper. Among them, the application of copper chromium arsenic preservative is more, and the chromium (Cr) therein has good fixation, but the side effect to the environment is very large. In comparison, ammonia soluble quaternary ammonium copper preservative not only has good antiseptic effect, but also is harmless to the environment, and therefore is widely recognized at home and abroad. China invention patent application publication number CN103283516A, application date is May 30, 2013, name is "Live tree poplar wood antiseptic treatment method", and the disclosed scheme includes the following process steps: 1) injection position of antiseptic liquid in the trunk, 2) antiseptic liquid concentration and injection amount, 3) determination of the initial time of injection of live tree poplar wood antiseptic liquid, 4) determination of poplar wood felling time, 5) inspection of the movement and penetration uniformity of the agent in the trunk, 6) inspection of poplar wood antiseptic performance. This scheme uses ammonia-soluble quaternary ammonium copper to treat live poplar trees. The negative pressure generated by the transpiration of the tree allows the ammonia-soluble quaternary ammonium copper to evenly penetrate all parts of the poplar. However, this scheme requires a long time to ensure that the preservative is evenly distributed in the trunk, affecting the treatment efficiency; the penetration of the preservative may lead to uneven distribution, especially in different parts of the tree. Since the production of oriented strand board usually involves directional laying and hot pressing of strands, it will affect the uniform penetration of the preservative. The hot pressing process may affect the chemical stability of the ammonia-soluble quaternary ammonium copper and reduce its anti-corrosion effect.
[0004] Compared with the pressure impregnation of solid trees / wood, the "separation-recombination" of wood units in oriented strand boards gives them more anti-corrosion treatment methods. For example, Jin Juwan et al. Effect of copper-based preservatives on the performance of bamboo oriented strand boards. Wood Industry [J]. 2009. 23 (5): 8-11. Wei Wanshu et al. Corrosion resistance of bamboo oriented strand boards treated with four preservatives. Wood Industry [J]. 2011. 25 (2): 8-10. They respectively disclose bamboo oriented strand boards treated with ammonia-dissolved quaternary ammonium copper. Since adhesives are used as raw materials in the production process of oriented strand boards, the above-mentioned prior art discloses that the type of adhesive may affect the anti-corrosion performance. Although the prior art uses ammonia-dissolved quaternary ammonium copper for live tree poplar or bamboo oriented strand boards to improve the anti-corrosion performance, for building material wood oriented strand boards, when stronger anti-corrosion performance is required, they must also be more environmentally friendly and safe to adapt to the increasing tendency of people to choose more environmentally friendly and safer glues and treatment agents for wood products. Summary of the invention
[0005] 1. Problems to be solved
[0006] When ammonia-soluble quaternary ammonium copper is used for wood preservation in the prior art, the anti-corrosion effect of ammonia-soluble quaternary ammonium copper increases with the increase in the amount of adhesive used, resulting in a large amount of adhesive used and a technical problem that is not environmentally friendly. The present application provides a method for preparing modified ammonia-soluble quaternary ammonium copper, and the prepared modified ammonia-soluble quaternary ammonium copper can enhance the anti-corrosion performance with a smaller amount of adhesive used. The present application also provides an anti-corrosion oriented strand board and a method for preparing the same, which has a simple preparation process, enhanced anti-corrosion ability, and can adapt to the existing production process and process of oriented strand boards.
[0007] 2. Technical solution
[0008] In order to achieve the above purpose, the technical solution provided is:
[0009] The preparation method of modified ammonia-soluble quaternary ammonium copper comprises the following steps:
[0010] S1. Mixing a poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion and ammonia-soluble quaternary ammonium copper in a mass ratio of (1 to 2):10;
[0011] S2. Evaporate and concentrate to a mass concentration of 30-40%.
[0012] The modified ammonia-soluble quaternary ammonium copper is prepared according to the method.
[0013] The application of modified ammonia-soluble quaternary ammonium copper is to apply the modified ammonia-soluble quaternary ammonium copper to the preparation of anti-corrosion materials.
[0014] The method for preparing the anticorrosive oriented strand board, using modified ammonia-soluble quaternary ammonium copper, comprises the following steps:
[0015] Wood shavings: to prepare surface layer raw materials and core layer raw materials;
[0016] Preparing the surface layer or the core layer: adding a phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper to the surface layer raw material or the core layer raw material, stirring evenly to obtain the surface layer or the core layer, wherein the solid content of the phenolic resin adhesive is 43-50%; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounts for 6-12% and 2-6% of the absolute dry mass of the surface layer or the core layer, respectively;
[0017] Preparation of anti-corrosion oriented strand board: laying multiple surface layers, core layers and surface layers in a three-layer structure in sequence; laying the surface layer uniformly at an angle of 0 to 90 degrees to the horizontal direction with the fiber direction; laying the core layer at an angle of 0 to 90 degrees to the surface layer fiber direction with the fiber direction; hot pressing to obtain the anti-corrosion oriented strand board.
[0018] Furthermore, the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounts for 8% and 6% of the absolute dry mass of the surface layer or the core layer, respectively.
[0019] Furthermore, the number of layers of the surface layer: the core layer: the surface layer is (2-3): (4-6): (2-3).
[0020] Furthermore, the surface layer material has a length of 10 to 15 cm, a width of 6 to 10 cm, and a thickness of 0.5 to 0.6 mm; the core layer material has a length of 6 to 8 cm, a width of 2 to 3 cm, and a thickness of 0.5 to 0.6 mm.
[0021] Preferably, the moisture content of the surface layer raw material and the core layer raw material after drying is 2-4%.
[0022] Furthermore, the hot pressing temperature is 180-200° C., the pressure is 2.5-6.0 MPa, and the hot pressing factor is 0.75-1.0 min / mm.
[0023] Furthermore, it also includes the steps of curing, trimming and sanding after the hot pressing step.
[0024] The anti-corrosion oriented strand board is prepared by using the method.
[0025] 3. Beneficial effects
[0026] Compared with the existing known technology, the technical solution provided by the present invention has the following beneficial effects:
[0027] (1) The preparation method of the modified ammonia-soluble quaternary ammonium copper of the present invention uses a modifier of poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion. The modifier and the ammonia-soluble quaternary ammonium copper are mixed and evaporated and concentrated to obtain the modified ammonia-soluble quaternary ammonium copper. The preparation method is simple, easy to operate and highly efficient.
[0028] (2) The modified ammonia-soluble quaternary ammonium copper of the present invention has a higher anti-corrosion effect than ammonia-soluble quaternary ammonium copper, and can enhance the anti-corrosion performance with a lower amount of adhesive.
[0029] (3) The modified ammonia-soluble quaternary ammonium copper of the present invention is applied to the preparation of anti-corrosion materials, especially to the anti-corrosion function treatment of indoor furniture wood / bamboo products and building materials, which gives wood and bamboo materials efficient anti-corrosion performance and safety performance, and plays a long-term protective role on wood and bamboo materials.
[0030] (4) The method for preparing the anti-corrosion oriented strand board of the present invention uses modified ammonia-soluble quaternary ammonium copper as an anti-corrosion agent, has a simple preparation process, enhanced anti-corrosion ability, and can adapt to the existing production process and process of oriented strand board.
[0031] (5) The anti-corrosion oriented strand board of the present invention has high anti-corrosion performance, can reach a strong corrosion resistance level, and is more environmentally friendly and safe. Other mechanical performance parameters can meet the requirements of building materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the preparation process of the anti-corrosion oriented strand board of the present invention. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0034] Abbreviations
[0035] OSB: oriented strand board;
[0036] ACQ: Ammoniacal Copper Quaternary, ammoniacal copper quaternary;
[0037] CCA: Chromated Copper Arsenate, copper chromium arsenate;
[0038] PF:phenol-formaldehyde resin, phenolic resin.
[0039] The method for preparing the anticorrosive oriented strand board of the present application comprises the following steps:
[0040] S1. Wood shavings: prepare surface layer raw materials and core layer raw materials; the surface layer raw materials have a length of 10 to 15 cm, a width of 6 to 10 cm, and a thickness of 0.5 to 0.6 mm; the core layer raw materials have a length of 6 to 8 cm, a width of 2 to 3 cm, and a thickness of 0.5 to 0.6 mm. Send the surface layer raw materials and the core layer raw materials into a dryer for drying. The moisture content of the surface layer raw materials and the core layer raw materials is 2 to 4 wt%.
[0041] S2. Phenolic resin adhesive: The solid content of the phenolic resin adhesive is 43-50%.
[0042] S3. Preparation of modified ammonia-soluble quaternary ammonium copper: uniformly mix the modifier and ammonia-soluble quaternary ammonium copper in a mass ratio of (1-2):10, and concentrate to a mass concentration of 30-40% by rotary evaporator; the modifier is poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion.
[0043] S4. Prepare the surface layer: add phenolic resin adhesive and modified ammonia-soluble quaternary ammonium copper to the surface layer raw material; add the phenolic resin adhesive to the surface layer raw material while stirring the surface layer raw material, then spray the modified ammonia-soluble quaternary ammonium copper onto the surface of the surface layer raw material, continue to stir evenly, and obtain the surface layer; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper account for 6-12% and 2-6% of the absolute dry mass of the surface layer, respectively.
[0044] S5. Prepare the core layer: add phenolic resin adhesive and modified ammonia-soluble quaternary ammonium copper to the core layer raw material; add the phenolic resin adhesive to the core layer raw material while stirring the core layer raw material, then spray the modified ammonia-soluble quaternary ammonium copper onto the surface of the core layer raw material, continue to stir evenly, and obtain the core layer; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper account for 6-12% and 2-6% of the absolute dry mass of the core layer, respectively.
[0045] S6. Directed paving: The three-layer structure is paved in the order of surface layer, core layer, and surface layer; the surface layer is evenly paved with the fiber direction at an angle of 0 to 90 degrees to the horizontal direction; the core layer is paved with the fiber direction at an angle of 0 to 90 degrees to the surface layer fiber direction; the mass ratio of the surface layer: core layer: surface layer is (2 to 3): (4 to 6): (2 to 3).
[0046] S7. Pre-press and hot-press to obtain anti-corrosion oriented strand board. The hot-pressing temperature is 180-200°C, the pressure is 2.5-6.0 MPa, and the hot-pressing factor is 0.75-1 min / mm. After pre-pressing and hot-pressing, curing, trimming and sanding are performed.
[0047] In the following examples, the poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion is composited by a poly(styrene-butyl acrylate-acrylic acid) emulsion having a solid content of 30 to 50% and a silicon dioxide nanocomposite emulsion having a solid content of 50 to 65%, wherein the solid content of the poly(styrene-butyl acrylate-acrylic acid) and the silicon dioxide nanocomposite is (10 to 20):15.
[0048] Example 1 (phenolic resin 8wt%; modified ammonia-soluble quaternary ammonium copper 6wt%)
[0049] The modified ammonia-soluble quaternary ammonium copper and anticorrosive oriented strand board, preparation method and application of this embodiment are as follows:
[0050] S1. Wood shavings: Prepare surface layer raw materials and core layer raw materials; the surface layer raw materials are 13 cm long, 8 cm wide, and 0.55 mm thick; the core layer raw materials are 7 cm long, 2.5 cm wide, and 0.55 mm thick. Send the surface layer raw materials and the core layer raw materials into a dryer for drying to a moisture content of 3 wt%.
[0051] S2. Preparation of phenolic resin adhesive: phenolic resin adhesive solid content 47%;
[0052] S3. Preparation of modified ammonia-soluble quaternary ammonium copper: The poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion modifier and the ammonia-soluble quaternary ammonium copper are uniformly mixed in a mass ratio of 1.5:10, and concentrated to a mass concentration of 35% by a rotary evaporator. The poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion is composed of a poly(styrene-butyl acrylate-acrylic acid) emulsion with a solid content of 40% and a silicon dioxide nanocomposite emulsion with a solid content of 58%, wherein the solid content of poly(styrene-butyl acrylate-acrylic acid) and silicon dioxide nanocomposite is 1:1.
[0053] S4. Preparation of the surface layer: adding a phenolic resin adhesive and a modified ammonia-soluble quaternary ammonium copper to the surface raw material; while stirring the surface raw material, adding the phenolic resin adhesive to the surface raw material, and then spraying the modified ammonia-soluble quaternary ammonium copper onto the surface of the surface raw material, continuing to stir evenly to obtain a surface layer; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounted for 8% and 6% of the absolute dry mass of the surface layer, respectively;
[0054] S5. Preparing a core layer: adding a phenolic resin adhesive and a modified ammonia-soluble quaternary ammonium copper to the core layer raw material; while stirring the core layer raw material, adding the phenolic resin adhesive to the core layer raw material, and then spraying the modified ammonia-soluble quaternary ammonium copper onto the surface of the core layer raw material, and continuing to stir evenly to obtain a core layer; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounted for 8% and 6% of the absolute dry mass of the core layer, respectively;
[0055] S6. Directional paving: The three-layer structure is laid in the order of surface layer, core layer, and surface layer; the surface layer is laid evenly with the fiber direction at 60° to the horizontal direction; the core layer is laid with the fiber direction at 90° to the fiber direction of the surface layer; the mass ratio of surface layer: core layer: surface layer is 2:5:2;
[0056] S7. Pre-press and hot-press to obtain the anti-corrosion oriented strand board. The hot-pressing temperature is 190°C, the pressure is 4.5MPa, and the hot-pressing factor is 0.85min / mm. After pre-press and hot-press, curing, trimming and sanding are performed.
[0057] The properties of the anti-corrosion oriented strand board prepared in this example are shown in Table 1.
[0058] Example 2 (phenolic resin 6wt%, modified ammonia-soluble quaternary ammonium copper 2wt%)
[0059] The modified ammonia-soluble quaternary ammonium copper and anticorrosive oriented strand board, preparation method and application of this embodiment are as follows:
[0060] S1. Wood shavings: Prepare surface layer raw materials and core layer raw materials; the surface layer raw materials are 10 cm long, 6 cm wide, and 0.5 mm thick; the core layer raw materials are 6 cm long, 2 cm wide, and 0.5 mm thick. Send the surface layer raw materials and the core layer raw materials into a dryer for drying to a moisture content of 2wt%.
[0061] S2. Preparation of phenolic resin adhesive: phenolic resin adhesive solid content 43%;
[0062] S3. Preparation of modified ammonia-soluble quaternary ammonium copper: poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion modifier and ammonia-soluble quaternary ammonium copper are uniformly mixed in a mass ratio of 1:10, and concentrated to a mass concentration of 33% by a rotary evaporator. The poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion is composed of a poly(styrene-butyl acrylate-acrylic acid) emulsion with a solid content of 30% and a silicon dioxide nanocomposite emulsion with a solid content of 50%, wherein the solid content of poly(styrene-butyl acrylate-acrylic acid) and silicon dioxide nanocomposite is 4:3.
[0063] S4. Preparation of the surface layer: adding a phenolic resin adhesive and a modified ammonia-soluble quaternary ammonium copper to the surface raw material; while stirring the surface raw material, adding the phenolic resin adhesive to the surface raw material, and then spraying the modified ammonia-soluble quaternary ammonium copper onto the surface of the surface raw material, continuing to stir evenly to obtain a surface layer; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounted for 6% and 2% of the absolute dry mass of the surface layer, respectively;
[0064] S5. Preparing a core layer: adding a phenolic resin adhesive and a modified ammonia-soluble quaternary ammonium copper to the core layer raw material; while stirring the core layer raw material, adding the phenolic resin adhesive to the core layer raw material, and then spraying the modified ammonia-soluble quaternary ammonium copper onto the surface of the core layer raw material, and continuing to stir evenly to obtain a core layer; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounted for 6% and 2% of the absolute dry mass of the core layer, respectively;
[0065] S6. Directional paving: The three-layer structure is laid in the order of surface layer, core layer, and surface layer; the surface layer is laid evenly with the fiber direction at 60° to the horizontal direction; the core layer is laid with the fiber direction at 90° to the fiber direction of the surface layer; the mass ratio of surface layer: core layer: surface layer is 2:4:3;
[0066] S7. Pre-press and hot-press to obtain anti-corrosion oriented strand board. The hot-pressing temperature is 180°C, the pressure is 2.5MPa, and the hot-pressing factor is 0.75min / mm. After pre-press and hot-press, curing, trimming and sanding are performed.
[0067] The properties of the anti-corrosion oriented strand board prepared in this example are shown in Table 1.
[0068] Example 3 (phenolic resin 12wt%, modified ammonia-soluble quaternary ammonium copper 4wt%)
[0069] The modified ammonia-soluble quaternary ammonium copper and anticorrosive oriented strand board, preparation method and application of this embodiment are as follows:
[0070] S1. Wood shavings: Prepare surface layer raw materials and core layer raw materials; the surface layer raw materials are 15 cm long, 10 cm wide, and 0.6 mm thick; the core layer raw materials are 8 cm long, 3 cm wide, and 0.6 mm thick. Send the surface layer raw materials and the core layer raw materials into a dryer for drying to a moisture content of 4 wt%.
[0071] S2. Preparation of phenolic resin adhesive: phenolic resin adhesive solid content 50%;
[0072] S3. Preparation of modified ammonia-soluble quaternary ammonium copper: poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion modifier and ammonia-soluble quaternary ammonium copper are uniformly mixed in a mass ratio of 1:5, and concentrated to a mass concentration of 40% by a rotary evaporator. The poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion is composed of a poly(styrene-butyl acrylate-acrylic acid) emulsion with a solid content of 50% and a silicon dioxide nanocomposite emulsion with a solid content of 65%, wherein the solid content of poly(styrene-butyl acrylate-acrylic acid) and silicon dioxide nanocomposite is 2:3.
[0073] S4. Preparation of the surface layer: adding a phenolic resin adhesive and a modified ammonia-soluble quaternary ammonium copper to the surface raw material; while stirring the surface raw material, adding the phenolic resin adhesive to the surface raw material, and then spraying the modified ammonia-soluble quaternary ammonium copper onto the surface of the surface raw material, continuing to stir evenly to obtain a surface layer; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounted for 12% and 4% of the absolute dry mass of the surface layer, respectively;
[0074] S5. Preparing the core layer: adding a phenolic resin adhesive and a modified ammonia-soluble quaternary ammonium copper to the core layer raw material; while stirring the core layer raw material, adding the phenolic resin adhesive to the core layer raw material, and then spraying the modified ammonia-soluble quaternary ammonium copper onto the surface of the core layer raw material, and continuing to stir evenly to obtain the core layer; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounted for 12% and 4% of the absolute dry mass of the core layer, respectively;
[0075] S6. Directional paving: The three layers are laid in the order of surface layer, core layer, and surface layer; the surface layer is laid evenly with the fiber direction at 60° to the horizontal direction; the core layer is laid with the fiber direction at 90° to the fiber direction of the surface layer; the mass ratio of surface layer: core layer: surface layer is 3:6:2;
[0076] S7. Pre-press and hot-press to obtain anti-corrosion oriented strand board. The hot-pressing temperature is 200°C, the pressure is 6.0 MPa, and the hot-pressing factor is 1.0 min / mm. After pre-pressing and hot-pressing, curing, trimming and sanding are performed.
[0077] The properties of the anti-corrosion oriented strand board prepared in this example are shown in Table 1.
[0078] Comparative Example 1 (phenolic resin 8wt%, ammonia-soluble quaternary ammonium copper 6wt%)
[0079] This comparative example is basically the same as Example 1, except that unmodified ammonia-soluble quaternary ammonium copper is used.
[0080] The properties of the anti-corrosion oriented strand board prepared in this comparative example are shown in Table 1.
[0081] Comparative Example 2 (10 wt% phenolic resin, 6 wt% ammonia-soluble quaternary ammonium copper)
[0082] This comparative example is basically the same as comparative example 1, except that the phenolic resin adhesive accounts for the mass of the absolute dry wood shavings.
[0083] The properties of the anti-corrosion oriented strand board prepared in this comparative example are shown in Table 1.
[0084] Comparative Example 3 (phenolic resin 8wt%, ammonia-soluble quaternary ammonium copper 4wt%)
[0085] This comparative example is basically the same as comparative example 1, except that the phenolic resin adhesive and ammonia-soluble quaternary ammonium copper account for the mass of the absolute dry wood shavings.
[0086] The properties of the anti-corrosion oriented strand board prepared in this comparative example are shown in Table 1.
[0087] Comparative Example 4 (phenolic resin 8wt%, ammonia-soluble quaternary ammonium copper 2wt%)
[0088] This comparative example is basically the same as comparative example 1, except that the phenolic resin adhesive and ammonia-soluble quaternary ammonium copper account for the mass of the absolute dry wood shavings.
[0089] The properties of the anti-corrosion oriented strand board prepared in this comparative example are shown in Table 1.
[0090] Comparative Example 5 (8 wt% phenolic resin, no ammonia-soluble quaternary ammonium copper)
[0091] This comparative example is basically the same as comparative example 1, except that no ammonia-soluble quaternary ammonium copper preservative is added.
[0092] The properties of the anti-corrosion oriented strand board prepared in this comparative example are shown in Table 1.
[0093] Comparative Example 6 (6 wt% phenolic resin, no ammonia-soluble quaternary ammonium copper)
[0094] This comparative example is basically the same as comparative example 1, except that the amount of phenolic resin adhesive added is 6wt%, and no ammonia-soluble quaternary ammonium copper preservative is added.
[0095] The properties of the anti-corrosion oriented strand board prepared in this comparative example are shown in Table 1.
[0096] Comparative Example 7 (phenolic resin 8wt%; ammonia-soluble quaternary ammonium copper and modifier 6wt% in total)
[0097] This comparative example is basically the same as Example 1, except that the ammonia-soluble quaternary ammonium copper is not modified, but is sprayed onto the surface of the wood chips separately with the modifier.
[0098] The properties of the anti-corrosion oriented strand board prepared in this comparative example are shown in Table 1.
[0099] The parameters of the oriented strand boards prepared in Examples 1-3 and Comparative Examples 1-7 are compared in Table 1.
[0100] Table 1 Performance parameters of anti-corrosion oriented strand board
[0101]
[0102] Note: According to GB / T 13942.1-2009 standard, the mass loss of 0-10% is the strong corrosion resistance grade; the mass loss of 11-24% is the corrosion resistance grade.
[0103] It can be seen from Examples 1-3 that when the addition amount of the phenolic resin adhesive is 6-12wt% and the addition amount of the modified ammonia-soluble quaternary ammonium copper is 2-6wt%, the mass loss rate of the oriented strand board is 1.63-6.03%, reaching a strong corrosion resistance grade. The mass loss rates of the oriented strand boards of Examples 1 and 3 are 1.63% and 1.70%, respectively, and the addition amounts of the phenolic resin adhesive are 8wt% and 12wt%, respectively. Considering the cost and environmental safety comprehensively, the technical scheme of Example 1 is the preferred scheme.
[0104] It can be seen from the comparative examples that, when the amount of phenolic resin adhesive added is the same, increasing the amount of ammonia-soluble quaternary ammonium copper added will reduce the mass loss rate of the oriented strand board. In comparative examples 4, 3, and 1, the amount of phenolic resin adhesive added is 8wt%, and the amount of ammonia-soluble quaternary ammonium copper added is 2wt%, 4wt%, and 6wt%, respectively. The mass loss rates of the final oriented strand board are 7.06wt%, 4.60wt%, and 2.53wt%, respectively.
[0105] When no ammonia-soluble quaternary ammonium copper is added, the mass loss rate of the oriented strand board decreases by increasing the amount of phenolic resin adhesive added. In comparative examples 6 and 5, no ammonia-soluble quaternary ammonium copper is added, the amount of phenolic resin adhesive added is 6wt% and 8wt%, respectively, and the mass loss rate of the oriented strand board is 11.2wt% and 7.58wt%, respectively.
[0106] It can be seen from the examples and comparative examples that in terms of anticorrosion performance, when the same amount of preservative is added, the modified ammonia-soluble quaternary ammonium copper has a better anticorrosion effect than the ammonia-soluble quaternary ammonium copper. Example 1 adds 6wt% of the modified ammonia-soluble quaternary ammonium copper, and the mass loss rate of the oriented strand board is 1.63wt%, and Comparative Example 1 adds 6wt% of the ammonia-soluble quaternary ammonium copper, and the mass loss rate of the oriented strand board is 2.53wt%. Comparative Example 7 first adds ammonia-soluble quaternary ammonium copper, and then adds the modifier, and the two add 6wt% in total, and the mass loss rate of the oriented strand board is 1.95%.
[0107] In terms of the amount of adhesive added, excellent anti-corrosion performance can be obtained while reducing the amount of adhesive used. Example 1 adds 6wt% of modified ammonia-soluble quaternary ammonium copper and 8wt% of phenolic resin adhesive, and the mass loss rate of the oriented strand board is 1.63wt%. Comparative Example 2 adds 6wt% of ammonia-soluble quaternary ammonium copper and 10wt% of phenolic resin adhesive, and the mass loss rate of the oriented strand board is 1.72wt%.
[0108] The above-mentioned embodiments only express the preferred implementation modes of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person skilled in the art, several modifications, improvements and substitutions can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the attached claims.
Claims
1. A method for preparing modified ammonia-soluble quaternary ammonium copper, characterized in that: The following steps are involved: S1. Mixing a poly(styrene-butyl acrylate-acrylic acid) / silicon dioxide nanocomposite emulsion and ammonia-soluble quaternary ammonium copper in a mass ratio of (1 to 2):10; S2. Evaporate and concentrate to a mass concentration of 30-40%.
2. Modified ammonia-soluble quaternary ammonium copper, characterized in that: Prepared according to the method of claim 1.
3. The application of modified ammonia-soluble quaternary ammonium copper is characterized by: The modified ammonia-soluble quaternary ammonium copper described in claim 2 is applied to the preparation of anti-corrosion materials.
4. A method for preparing an anticorrosive oriented strand board, characterized in that: Using the modified ammonia-soluble quaternary ammonium copper according to claim 2 comprises the following steps: Wood shavings: to prepare surface layer raw materials and core layer raw materials; Preparing the surface layer or the core layer: adding a phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper to the surface layer raw material or the core layer raw material, stirring evenly to obtain the surface layer or the core layer, wherein the solid content of the phenolic resin adhesive is 43-50%; the solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounts for 6-12% and 2-6% of the absolute dry mass of the surface layer or the core layer, respectively; Preparation of anti-corrosion oriented strand board: laying multiple surface layers, core layers and surface layers in a three-layer structure in sequence; laying the surface layer uniformly at an angle of 0 to 90 degrees to the horizontal direction with the fiber direction; laying the core layer at an angle of 0 to 90 degrees to the surface layer fiber direction with the fiber direction; hot pressing to obtain the anti-corrosion oriented strand board.
5. The method for preparing the anticorrosive oriented strand board according to claim 4, characterized in that: The solid mass of the phenolic resin adhesive and the modified ammonia-soluble quaternary ammonium copper accounts for 8% and 6% of the absolute dry mass of the surface layer or the core layer respectively.
6. The method for preparing the anticorrosive oriented strand board according to claim 5, characterized in that: The number of layers of the surface layer: the core layer: the surface layer is (2-3): (4-6): (2-3).
7. The method for preparing the anticorrosive oriented strand board according to claim 6, characterized in that: The surface layer material has a length of 10 to 15 cm, a width of 6 to 10 cm, and a thickness of 0.5 to 0.6 mm; the core layer material has a length of 6 to 8 cm, a width of 2 to 3 cm, and a thickness of 0.5 to 0.6 mm.
8. The method for preparing the anticorrosive oriented strand board according to claim 7, characterized in that: The hot pressing temperature is 180-200° C., the pressure is 2.5-6.0 MPa, and the hot pressing factor is 0.75-1.0 min / mm.
9. The method for preparing the anticorrosive oriented strand board according to any one of claims 4 to 8, characterized in that: The method also includes the steps of curing, trimming and sanding after the hot pressing step.
10. Anticorrosive oriented strand board, characterized by: It is prepared by the method according to any one of claims 4 to 9.
Citation Information
Patent Citations
Manufacturing method for bamboo scrimber with outdoor weatherability
CN105538473A
Process method for modifying preservative treatment material based on nanometer silicon dioxide and emulsified wax
CN108032393A
Preparation method of high-moisture-proof bamboo shaving board
CN116277323A
Wooden modifying composition, production and use thereof
CN1644334A
Antiseptic treatment method of wood
JP2000238011A
Cited By
Preparation method of anti-corrosion high-strength OSB (oriented strand board)-based laminated wood