Lithium iron phosphate precursor and preparation method thereof, and carbon-coated lithium iron phosphate and preparation method thereof

By pre-synthesizing lithium iron phosphate precursor and carbon coating treatment, the inconsistent performance of lithium iron phosphate materials caused by uneven kiln temperature is solved, and the preparation of high consistency and high performance carbon-coated lithium iron phosphate materials is achieved.

CN118877853APending Publication Date: 2024-11-01DONGGUAN DONGYANG SOLAR SCI RES & DEV CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410909130.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

During the calcination process, the existing lithium iron phosphate process leads to inconsistent material performance due to uneven kiln temperature, which affects the capacity and rate performance of large-scale production of lithium iron phosphate materials.

Method used

By pre-synthesizing lithium iron phosphate precursors and adding carbon coating to industrial production to control the internal temperature of the kiln, avoid temperature differences, and improve material consistency and performance. The specific method includes adjusting the pH value of the source solution, adding a carbon source for liquid phase reaction, and then washing with a weakly alkaline solution to remove heteroatoms and forming iron vacancy to ensure that the crystals are equilibrium during high temperature sintering.

Benefits of technology

The high consistency and high performance of carbon-coated lithium iron phosphate material is achieved, the content of inactive materials is reduced, the capacity and rate performance of the material are improved, and the data fluctuations between batches are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004933031670000131
    Figure BDA0004933031670000131
Patent Text Reader

Abstract

The invention relates to the technical field of lithium batteries, and relates to a lithium iron phosphate precursor and a preparation method thereof, and carbon-coated lithium iron phosphate and a preparation method thereof. A lithium iron phosphate precursor which is uniform in phase and has iron vacancies on the surface is synthesized, and the precursor is added into a lithium iron phosphate raw material for industrial production, so that product performance difference caused by temperature difference in a kiln can be avoided under the condition that existing equipment is insufficient; the content of a non-active material in the carbon-coated lithium iron phosphate material is reduced, and the consistency of the carbon-coated lithium iron phosphate material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a lithium iron phosphate precursor and a preparation method thereof, and a carbon-coated lithium iron phosphate and a preparation method thereof. Background Art

[0002] At present, the mass production of lithium iron phosphate process mostly adopts iron phosphate and lithium carbonate mixed sand grinding and then sintering, and the sintering equipment mostly adopts roller kiln. Due to the structure of roller kiln, there will be uneven temperature inside the kiln during the calcination process. When mass production is carried out, in order to reduce production costs, multiple batches of feeding are required, which further leads to temperature fluctuations in the kiln, easily forming impurities, affecting the consistency of lithium iron phosphate, and reducing the performance of lithium iron phosphate materials. Specifically, when the local sintering temperature inside the kiln is too high, the melting effect between the particles is enhanced, forming large particles, increasing the diffusion distance of lithium ions, and reducing the capacity and rate performance of lithium iron phosphate materials; when the local sintering temperature inside the kiln is too low, the added precursor cannot completely react to form the target lithium iron phosphate, resulting in a decrease in the proportion of active materials and a reduction in the discharge capacity of lithium iron phosphate materials; due to the uneven sintering temperature inside the kiln, the synthesized lithium iron phosphate material is also uneven. After the lithium iron phosphate material is prepared into batteries in large quantities, the data fluctuations between batches are large, which affects the subsequent use of batteries.

[0003] Therefore, there is an urgent need to provide a method for preparing lithium iron phosphate that is suitable for production conditions in a wide temperature range. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the present invention provides a lithium iron phosphate precursor and a preparation method, a carbon-coated lithium iron phosphate and a preparation method. By pre-synthesizing a lithium iron phosphate precursor and adding it to the industrially produced lithium iron phosphate raw material, this method can avoid the difference in product performance caused by the temperature difference inside the kiln under the objective condition that the current equipment is insufficient, reduce the content of inactive materials in the carbon-coated lithium iron phosphate material, and improve the consistency of the carbon-coated lithium iron phosphate material.

[0005] To this end, the first aspect of the present invention provides a method for preparing a lithium iron phosphate precursor, comprising:

[0006] preparing a first lithium source solution, a first iron source solution, and a first phosphorus source solution, and adjusting the pH values ​​of the first lithium source solution, the first iron source solution, and the first phosphorus source solution to be less than 4.0;

[0007] Mixing the first lithium source solution, the first iron source solution, and the first phosphorus source solution to obtain a mixed solution a;

[0008] Adjusting the pH value of the mixed solution a until a precipitate is generated in the mixed solution a to obtain a mixed solution b;

[0009] Controlling the pH value of the mixed solution b to increase by 0.01-0.1 per minute, adjusting the pH value of the mixed solution b to 5.0-5.5, to obtain a mixed solution c;

[0010] Adding a first carbon source to the mixed solution c for liquid phase reaction to obtain lithium iron phosphate crystals;

[0011] The lithium iron phosphate crystals are washed with a weak alkaline solution to obtain the lithium iron phosphate precursor.

[0012] To solve the deficiencies in the prior art, the present invention avoids the generation of inhomogeneous phases during the preparation of lithium iron phosphate precursors by controlling the pH value of the source solution and the pH value change rate of the mixed solution a. At the same time, the addition of the first carbon source can improve the conductivity of the lithium iron phosphate precursor, and then wash it with a weak alkaline solution (such as at least one of an ammonia solution, an ethylenediamine solution, a triethanolamine solution, an aniline solution, and an alkyl alcoholamine solution), which can clean the heteroatoms. At the same time, since the weak alkaline solution has a certain complexing effect on iron ions, iron vacancies can be manufactured on the surface of the prepared lithium iron phosphate precursor by washing with a weak alkaline solution, and the manufactured iron vacancies avoid the melting of particles caused by the same crystal plane potential energy. Due to the lack of some atoms, the overall lattice of the lithium iron phosphate precursor is in a mismatched state, and the crystal is in an unbalanced state. It needs to react to a balanced state under high-temperature sintering, so it will absorb more heat in the subsequent preparation process of lithium iron phosphate, thereby balancing the temperature inside the entire kiln, so that the carbon-coated lithium iron phosphate product has better consistency.

[0013] According to an embodiment of the present invention, the first lithium source in the first lithium source solution includes at least one selected from lithium sulfate, lithium acetate, lithium nitrate, lithium gluconate, lithium chloride, lithium hydroxide, and lithium fluoride.

[0014] According to an embodiment of the present invention, the first iron source in the first iron source solution includes at least one selected from ferrous sulfate, ferric nitrate, ferric gluconate, ferrous chloride, and ferric fluoride.

[0015] According to an embodiment of the present invention, the first phosphorus source in the first phosphorus source solution includes at least one selected from phosphoric acid, ammonium monohydrogen phosphate, and ammonium dihydrogen phosphate.

[0016] According to an embodiment of the present invention, the first lithium source solution, the first iron source solution, and the first phosphorus source solution are mixed according to an element molar ratio of Li:Fe:P of (1.0-1.05):(0.95-1):1.

[0017] According to an embodiment of the present invention, the first carbon source includes at least one selected from dopamine hydrochloride, glucose, gluconolactone, and polyethylene glycol; wherein at least dopamine hydrochloride is included.

[0018] According to an embodiment of the present invention, the molar ratio of the first carbon source to the first phosphorus source is (0.01-0.2):1.

[0019] According to an embodiment of the present invention, the temperature of the liquid phase reaction is 80-180°C.

[0020] According to an embodiment of the present invention, the liquid phase reaction time is 8-36 hours.

[0021] According to an embodiment of the present invention, the weak alkaline solution is at least one of an aqueous ammonia solution, an ethylenediamine solution, a triethanolamine solution, an aniline solution, and an alkyl alcoholamine solution.

[0022] According to an embodiment of the present invention, the concentration of the weak alkaline solution is 0.1-2 mol / L.

[0023] A second aspect of the present invention provides a lithium iron phosphate precursor, which is obtained according to the preparation method described in the first aspect.

[0024] The lithium iron phosphate precursor obtained according to the above-mentioned preparation method has a relatively uniform physical phase. At the same time, during the preparation process, the iron atoms on the surface of the lithium iron phosphate precursor are dissolved by washing with a weak alkaline solution (such as at least one of an ammonia solution, an ethylenediamine solution, a triethanolamine solution, an aniline solution, and an alkyl alcoholamine solution), and part of the iron element is removed, resulting in the lack of iron elements on the outer surface of the lithium iron phosphate precursor, thereby avoiding melting during high-temperature sintering, thereby avoiding the formation of large particles. At the same time, due to the lack of some atoms, the overall lattice of the lithium iron phosphate precursor is in a mismatched state, and it needs to react to an equilibrium state under high-temperature sintering, so it absorbs more heat under high-temperature sintering, thereby balancing the temperature inside the entire kiln, so that the carbon-coated lithium iron phosphate product has better consistency.

[0025] A third aspect of the present invention provides a method for preparing carbon-coated lithium iron phosphate, the preparation method comprising:

[0026] Mixing a lithium iron phosphate precursor with a second lithium source, a second iron source, a second phosphorus source, and a second carbon source, and sintering to obtain the carbon-coated lithium iron phosphate;

[0027] Wherein, the lithium iron phosphate precursor is obtained according to the preparation method described in the first aspect or is the lithium iron phosphate precursor described in the second aspect.

[0028] In the industrial production of lithium iron phosphate, a highly consistent and high-performance carbon-coated lithium iron phosphate can be synthesized by adding the lithium iron phosphate precursor prepared above. Since the lithium iron phosphate precursor is a lithium iron phosphate crystal, the lithium iron phosphate raw material before sintering (referring to: the second lithium source, the second iron source, the second phosphorus source, the second carbon source, excluding the lithium iron phosphate precursor) is a mixture of multiple components. Under the current sintering process, the lithium iron phosphate precursor does not react too much with the raw materials, thereby maintaining its original shape. At the same time, the lithium iron phosphate precursor can prevent the melting of industrial lithium iron phosphate particles at high temperatures, reduce the particle size and the distance that lithium ions migrate within the particles, thereby improving the performance of the obtained carbon-coated lithium iron phosphate material.

[0029] According to an embodiment of the present invention, the second lithium source includes at least one selected from lithium carbonate, lithium phosphate, and lithium oxalate.

[0030] According to an embodiment of the present invention, the second iron source includes at least one selected from ferric phosphate, ferrous phosphate, iron oxide, and ferrous oxalate.

[0031] According to an embodiment of the present invention, the second phosphorus source includes at least one selected from iron phosphate, ammonium dihydrogen phosphate, and lithium hydrogen phosphate.

[0032] According to an embodiment of the present invention, the second carbon source includes at least one selected from glucose, ethylene glycol, toluene, n-octane, and ethyl acetate.

[0033] According to an embodiment of the present invention, the second lithium source, the second iron source, and the second phosphorus source are mixed according to an element molar ratio of Li:Fe:P of (1-1.05):1:(1-1.05).

[0034] According to an embodiment of the present invention, the molar ratio of the lithium iron phosphate precursor to the iron element in the second lithium source, the second iron source, the second phosphorus source, and the second carbon source is 0.01-0.1:1.

[0035] According to an embodiment of the present invention, the molar ratio of the second carbon source to the lithium iron phosphate precursor is 1 to 10:1.

[0036] A fourth aspect of the present invention provides a carbon-coated lithium iron phosphate, wherein the carbon-coated lithium iron phosphate is obtained according to the preparation method described in the third aspect.

[0037] Therefore, the carbon-coated lithium iron phosphate has high consistency and high performance.

[0038] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION

[0039] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be understood as limiting the present invention.

[0040] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Further, in the description of the present invention, unless otherwise specified, the meaning of "plurality" is two or more.

[0041] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0042] In order to make the present invention more easily understood, certain technical and scientific terms are specifically defined below. Unless otherwise clearly defined elsewhere in this document, all other technical and scientific terms used herein have the meanings commonly understood by those skilled in the art to which the present invention belongs.

[0043] In this document, the terms “include” or “comprising” are open expressions, that is, including the contents specified in the present invention but not excluding other contents.

[0044] As used herein, the terms "optionally", "optional" or "optionally" generally mean that the subsequently described event or circumstance may but need not occur, and that the description includes instances where the event or circumstance occurs and instances where it does not.

[0045] According to an embodiment of the present invention, a method for preparing a lithium iron phosphate precursor in a first aspect of the present invention comprises:

[0046] (1) preparing a first lithium source solution, a first iron source solution, and a first phosphorus source solution, and adjusting the pH values ​​of the first lithium source solution, the first iron source solution, and the first phosphorus source solution to be less than 4.0.

[0047] According to a specific embodiment of the present invention, the type of the first lithium source in the first lithium source solution is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, the first lithium source includes but is not limited to lithium sulfate, lithium acetate, lithium nitrate, lithium gluconate, lithium chloride, lithium hydroxide, and lithium fluoride.

[0048] According to a specific embodiment of the present invention, the type of the first iron source in the first iron source solution is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, the first iron source includes but is not limited to ferrous sulfate, ferric nitrate, ferric gluconate, ferrous chloride, and ferric fluoride.

[0049] According to a specific embodiment of the present invention, the type of the first phosphorus source in the first phosphorus source solution is not particularly limited, and those skilled in the art may select it according to actual needs. As some specific examples, the first phosphorus source includes but is not limited to phosphoric acid, monoammonium hydrogen phosphate, and diammonium hydrogen phosphate.

[0050] According to a specific embodiment of the present invention, the pH value of the first lithium source solution, the first iron source solution, and the first phosphorus source solution should be less than 4.0. Thus, the uniform state of the solution is maintained to avoid the generation of precipitation in the solution, resulting in uneven distribution of subsequent reaction elements. If the pH value of the source solution exceeds 4.0, during the subsequent pH adjustment process, the solution system will be in a non-equilibrium state, and there are no large number of crystal nuclei in the solution. Due to the addition of the solution for adjusting the pH, a large number of non-target products will be produced locally, resulting in failure of the precursor preparation or more impurities.

[0051] Specifically, the preparation method of each source solution is not particularly limited, and those skilled in the art can choose according to actual needs. As some specific examples, a soluble lithium source, a soluble iron source, and a soluble phosphorus source can be respectively dissolved in deionized water to obtain corresponding source solutions, and an appropriate amount of acid solution is added to adjust the pH value of the source solution to less than 4.0. If the pH value of the source solution meets the requirements, acid adjustment is not required.

[0052] (2) The first lithium source solution, the first iron source solution, and the first phosphorus source solution are mixed to obtain a mixed solution a.

[0053] According to a specific embodiment of the present invention, the first lithium source, the first iron source, and the first phosphorus source are mixed according to an element molar ratio of Li:Fe:P of (1.0-1.05):(0.95-1):1. As some specific examples, they can be mixed according to an element molar ratio of Li:Fe:P of 1.0:1.0:1, 1.01:0.99:1, 1.02:0.98:1, 1.02:0.95:1, 1.0:0.95:1, 1.03:0.95:1, 1.04:0.95:1, 1.05:0.95:1, etc.

[0054] (3) adjusting the pH value of the mixed solution a until a precipitate is generated in the mixed solution a, thereby obtaining a mixed solution b.

[0055] According to a specific embodiment of the present invention, the pH value of the mixed solution a here can be adjusted by adding an alkaline solution to the solution until a precipitate is generated in the mixed solution a. The type of alkaline solution is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, the alkaline solution can be selected from ammonia water, sodium hydroxide solution, potassium hydroxide solution, lithium hydroxide solution, etc.

[0056] (4) Controlling the pH value of the mixed solution b to increase by 0.01-0.1 per minute, adjusting the pH value of the mixed solution b to 5.0-5.5, and obtaining a mixed solution c. As some specific examples, the pH value of the mixed solution b increases by 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 per minute; adjusting the pH value of the mixed solution b to 5.0, 5.1, 5.2, 5.3, 5.4, 5.5.

[0057] According to a specific embodiment of the present invention, the process needs to control the pH rising rate of the reaction system to allow crystal nuclei to form evenly in the system. However, too fast a change in pH value will lead to uneven local dispersion and produce non-target products, and the consistency and performance of the obtained lithium iron phosphate precursor will be poor.

[0058] (5) Adding a first carbon source to the mixed solution c to react in a liquid phase to obtain lithium iron phosphate crystals.

[0059] The addition of the first carbon source can improve the conductivity of the lithium iron phosphate precursor. The type of the first carbon source is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, the first carbon source can be selected from dopamine hydrochloride, glucose, gluconolactone, polyethylene glycol, etc.; wherein at least dopamine hydrochloride is included, and the molecular formula of dopamine hydrochloride is C8H 12ClNO2, after high-temperature sintering, the chloride ions are removed in the form of gas ions, and the residual carbon forms a nano-scale carbon coating on the lithium iron phosphate precursor, which can effectively prevent the precursor formed by lithium iron phosphate from melting with the mass-produced lithium iron phosphate, avoid the growth of particles, effectively reduce the diffusion path of lithium iron phosphate, and increase the capacity and rate performance of the product. In addition, there is nitrogen in the molecular formula of dopamine hydrochloride, which can in-situ dope the carbon formed after high-temperature sintering to improve the conductivity of the lithium iron phosphate precursor. At the same time, dopamine hydrochloride is easily soluble in water, and is in an acidic state after being dissolved in water. At the same time, it will not affect the synthesis of the lithium iron phosphate precursor during the reaction process. Due to the properties of dopamine hydrochloride, it will change from a solution state to a precipitate when the pH value changes. With the subsequent washing with a weak alkaline solution (such as at least one of an ammonia solution, an ethylenediamine solution, a triethanolamine solution, an aniline solution, and an alkyl alcoholamine solution), it can be evenly coated on the surface of the synthesized lithium iron phosphate precursor. At the same time, due to the coordination effect of chloride ions, the coating layer and the lithium iron phosphate precursor can be chemically bonded, thereby enhancing the comprehensive performance of the lithium iron phosphate precursor.

[0060] According to a specific embodiment of the present invention, the amount of the first carbon source added is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, the molar ratio of the first carbon source to the first phosphorus source is (0.01-0.2): 1. As some specific examples, the molar ratio of the first carbon source to the first phosphorus source is 0.01: 1, 0.02: 1, 0.03: 1, 0.04: 1, 0.05: 1, 0.06: 1, 0.07: 1, 0.08: 1, 0.09: 1, 0.1: 1, 0.11: 1, 0.12: 1, 0.13: 1, 0.14: 1, 0.15: 1, 0.16: 1, 0.17: 1, 0.18: 1, 0.19: 1, 0.2: 1.

[0061] According to a specific embodiment of the present invention, a first carbon source is added to the mixed solution c and then a liquid phase reaction is carried out. The temperature and time of the liquid phase reaction are not particularly limited, and those skilled in the art can select according to actual needs. As some specific examples, the liquid phase reaction can be carried out at 80-180°C, such as 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, etc. The reaction can be carried out for 8-36 hours, such as 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, 25h, 26h, 27h, 28h, 29h, 30h, 31h, 32h, 33h, 34h, 35h, 36h, etc.

[0062] (6) Washing the lithium iron phosphate crystals with a weak alkaline solution to obtain the lithium iron phosphate precursor.

[0063] The etching depth of iron ions on the surface of the lithium iron phosphate precursor can be changed by washing with a weak alkaline solution (such as at least one of ammonia solution, ethylenediamine solution, triethanolamine solution, aniline solution, and alkyl alcoholamine solution). At the same time, because the weak alkaline solution has a certain complexing effect on ferrous ions, the iron atoms on the surface of the lithium iron phosphate precursor will be dissolved during the washing process. By removing some iron elements, the iron elements on the outer surface of the lithium iron phosphate precursor are missing, which avoids the melting of the raw materials used in the current mass production of lithium iron phosphate process (referring to: the second lithium source, the second iron source, the second phosphorus source, the second carbon source, excluding the lithium iron phosphate precursor) during high-temperature sintering, and prevents the formation of large particles. At the same time, due to the lack of some atoms, the overall lattice of the lithium iron phosphate precursor is in a mismatched state, and the crystal is in an unbalanced state. It needs to react to the equilibrium state under high-temperature sintering, so it absorbs more heat under high-temperature sintering, thereby balancing the temperature inside the entire kiln, so that the obtained carbon-coated lithium iron phosphate product has better consistency.

[0064] According to a specific embodiment of the present invention, the weak alkaline solution may be at least one of an aqueous ammonia solution, an ethylenediamine solution, a triethanolamine solution, an aniline solution, and an alkyl alcoholamine solution.

[0065] In the present invention, the washing solution must be weakly alkaline to ensure that it can react with dopamine hydrochloride so that dopamine hydrochloride can be precipitated on the surface of the lithium iron phosphate precursor to form a carbon coating layer; and the solution needs to form a certain complexing effect on the iron ions so that the iron ions on the surface can be complexed to form vacancies.

[0066] According to a specific embodiment of the present invention, the concentration of the weak alkaline solution is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, the concentration of the weak alkaline solution can be selected from 0.1 to 2 mol / L, such as 0.1 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, etc., and the pH value of the weak alkaline solution is 9 to 10.

[0067] According to a specific embodiment of the present invention, the preparation method further comprises: washing the lithium iron phosphate crystals with a weak alkaline solution, and drying them under vacuum conditions for standby use. The drying temperature is not particularly limited, and can be selected from 90°C, 95°C, 100°C, 105°C, 110°C, etc.

[0068] A second aspect of the present invention provides a lithium iron phosphate precursor, which is obtained according to the preparation method described in the first aspect.

[0069] Thus, a lithium iron phosphate precursor with high consistency and high performance is obtained.

[0070] A third aspect of the present invention provides a method for preparing carbon-coated lithium iron phosphate, the preparation method comprising:

[0071] Mixing a lithium iron phosphate precursor with a second lithium source, a second iron source, a second phosphorus source, and a second carbon source, and sintering to obtain the carbon-coated lithium iron phosphate;

[0072] Wherein, the lithium iron phosphate precursor is prepared according to the preparation method described in the first aspect or is the lithium iron phosphate precursor described in the second aspect.

[0073] By adding the aforementioned lithium iron phosphate precursor to the industrial production of lithium iron phosphate, the production quality can be stabilized, the performance of carbon-coated lithium iron phosphate products can be improved, and a highly consistent and high-performance carbon-coated lithium iron phosphate positive electrode material can be synthesized. Since the lithium iron phosphate precursor is a lithium iron phosphate crystal, the lithium iron phosphate raw material before sintering (referring to: the second lithium source, the second iron source, the second phosphorus source, the second carbon source, excluding the lithium iron phosphate precursor) is a mixture of multiple components, so under the current sintering process, the lithium iron phosphate precursor does not react too much with the raw materials, thereby maintaining its original shape. Adding a lithium iron phosphate precursor can prevent the melting of industrial lithium iron phosphate particles at high temperatures, reduce the particle size, and reduce the distance that lithium ions migrate inside the particles, thereby improving the performance of the obtained carbon-coated lithium iron phosphate. If the aforementioned lithium iron phosphate precursor is not added, the electrical performance of the obtained carbon-coated lithium iron phosphate will be reduced due to the instability of the kiln during the sintering process. For example, a kiln has multiple saggers, and the material near the heating side will be at a higher temperature than the material in the center, causing differences in the consistency of the produced carbon-coated lithium iron phosphate and resulting in reduced performance.

[0074] According to a specific embodiment of the present invention, the type of the second lithium source is not particularly limited, and those skilled in the art may select it according to actual needs. As some specific examples, lithium carbonate, lithium phosphate, lithium oxalate, etc. may be selected.

[0075] According to a specific embodiment of the present invention, the type of the second iron source is not particularly limited, and those skilled in the art may select it according to actual needs. As some specific examples, ferric phosphate, ferrous phosphate, ferrous oxide, ferrous oxalate, etc. may be selected.

[0076] According to a specific embodiment of the present invention, the type of the second phosphorus source is not particularly limited, and those skilled in the art may select it according to actual needs. As some specific examples, iron phosphate, diammonium phosphate, lithium hydrogen phosphate, etc. may be selected.

[0077] According to a specific embodiment of the present invention, the type of the second carbon source is not particularly limited, and those skilled in the art may select it according to actual needs. As some specific examples, glucose, ethylene glycol, toluene, n-octane, ethyl acetate, etc. may be selected.

[0078] According to a specific embodiment of the present invention, the second lithium source, the second iron source, and the second phosphorus source are mixed according to the element molar ratio of Li:Fe:P of (1-1.05):1:(1-1.05). As some specific examples, Li:Fe:P is mixed in the range of 1.0:1:1.0, 1.01:1:1.01, 1.02:1:1.02, 1.02:1:1.05, 1.0:1:1.05, 1.03:1:1.0, 1.04:1:1.05, 1.05:1:1.05, etc.

[0079] According to a specific embodiment of the present invention, the molar ratio of the lithium iron phosphate precursor to the iron element in the second lithium source, the second iron source, the second phosphorus source, and the second carbon source is 0.01 to 0.1: 1. As some specific examples, the molar ratio of the lithium iron phosphate precursor to the iron element in the second lithium source, the second iron source, the second phosphorus source, and the second carbon source is 0.01: 1, 0.02: 1, 0.03: 1, 0.04: 1, 0.05: 1, 0.06: 1, 0.07: 1, 0.08: 1, 0.09: 1, 0.1: 1, etc.

[0080] According to a specific embodiment of the present invention, the molar ratio of the second carbon source to the lithium iron phosphate precursor is 1 to 10: 1. As some specific examples, the molar ratio of the second carbon source to the lithium iron phosphate precursor is 1: 1, 2: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1, 9: 1, 10: 1, etc.

[0081] According to a specific embodiment of the present invention, the sintering temperature is not particularly limited, and those skilled in the art can choose according to actual needs. As some specific examples, the sintering can be carried out at 680-840°C, such as 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C, etc.

[0082] According to a specific embodiment of the present invention, the sintering time is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, the sintering time can be 12-24 hours, such as 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, etc.

[0083] According to a specific embodiment of the present invention, the preparation method may also include: mixing and dissolving a second lithium source, a second iron source, a second phosphorus source, and a second carbon source in deionized water, adding the lithium iron phosphate precursor prepared above, mixing and crushing to a target particle size, drying and placing in a production line kiln for sintering in an inert gas environment, and cooling and crushing to obtain carbon-coated lithium iron phosphate.

[0084] A fourth aspect of the present invention provides a carbon-coated lithium iron phosphate, wherein the carbon-coated lithium iron phosphate is obtained according to the preparation method described in the third aspect.

[0085] The result is a highly consistent, high-performance carbon-coated lithium iron phosphate material.

[0086] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.

[0087] Example 1

[0088] 1. Weigh 5.2 mol of lithium sulfate, 9.8 mol of ferrous sulfate, and 10 mol of phosphoric acid and dissolve them in 10 L of deionized water (the pH value of the mixed solution is lower than 4.0 at this time, and there is no need to add acidic solution to adjust the pH value). Mix the three solutions to obtain a mixed solution ①;

[0089] 2. Quickly adjust the pH value of the mixed solution ① obtained in step 1 to 4, and then add lithium hydroxide solution to the solution at a rate of 0.01 pH value per minute to slowly increase the pH value to 5.0. Since there is a buffering process in the latter stage of the reaction to avoid the pH value being too high, lithium hydroxide solution is continued to be added after the pH value is higher than 5.0 and stabilized for 1 minute. When the pH value reaches 5.5, add 0.5 mol of dopamine hydrochloride. Place the above solution in a reactor and heat to 140°C for 24 hours;

[0090] 3. After the reaction in step 2 is completed, the undried lithium iron phosphate precursor ① obtained from the reactor is washed clean with 1 mol / L ammonia water, and vacuum dried at 110° C. to obtain a dried lithium iron phosphate precursor ① for standby use;

[0091] 4. Weigh 100 mol of iron phosphate, 52 mol of lithium carbonate, and 10 mol of glucose, mix and dissolve them in deionized water, add 5 mol of the dried lithium iron phosphate precursor ① obtained in step 3, and then mix the materials with a sand mill and grind them to D 50≤400nm. Then, the sand-milled material is formed into a mixed powder by spray drying, and the powder is placed in a production line kiln in an inert gas environment and sintered at 780°C for 16 hours, and then cooled and crushed to obtain a carbon-coated lithium iron phosphate finished product①.

[0092] Example 2

[0093] 1. Weigh 5.2 mol of lithium sulfate, 9.8 mol of ferrous sulfate, and 10 mol of phosphoric acid and dissolve them in 10 L of deionized water (the pH value of the mixed solution is lower than 4.0 at this time, and there is no need to add acidic solution to adjust the pH value). Mix the three solutions to obtain a mixed solution ②;

[0094] 2. Quickly adjust the pH value of the mixed solution ② obtained in step 1 to 4, and then add lithium hydroxide solution to the solution at a rate of 0.01 pH value per minute to slowly increase the pH value to 5.0. Since there is a buffering process in the latter stage of the reaction to avoid the pH value being too high, lithium hydroxide solution is continued to be added after the pH value is higher than 5.0 and stabilized for 1 minute. When the pH value reaches 5.5, add 0.5 mol of dopamine hydrochloride. Place the above solution in a reactor and heat to 140°C for 24 hours;

[0095] 3. After the reaction in step 2 is completed, the undried lithium iron phosphate precursor ② obtained from the reactor is washed clean with 0.1 mol / L ammonia water, and vacuum dried at 110° C. to obtain a dried lithium iron phosphate precursor ② for standby use;

[0096] 4. Weigh 100 mol of iron phosphate, 52 mol of lithium carbonate, and 10 mol of glucose, mix and dissolve them in deionized water, add 5 mol of the dried lithium iron phosphate precursor ② obtained in step 3, and then mix the materials with a sand mill and grind them to D 50 ≤400nm. Then, the sand-milled material is formed into a mixed powder by spray drying, and the powder is placed in a production line kiln in an inert gas environment and sintered at 780°C for 16 hours, and then cooled and crushed to obtain a carbon-coated lithium iron phosphate finished product②.

[0097] Example 3

[0098] 1. Weigh 5.2 mol of lithium sulfate, 9.8 mol of ferrous sulfate, and 10 mol of phosphoric acid and dissolve them in 10 L of deionized water (the pH value of the mixed solution is lower than 4.0 at this time, and there is no need to add acidic solution to adjust the pH value). Mix the three solutions to obtain a mixed solution ③;

[0099] 2. Quickly adjust the pH value of the mixed solution ③ obtained in step 1 to 4, and then add lithium hydroxide solution to the solution at a rate of 0.01 pH value per minute to slowly increase the pH value to 5.0. Since there is a buffering process in the latter stage of the reaction to avoid the pH value being too high, lithium hydroxide solution is continued to be added after the pH value is higher than 5.0 and stabilized for 1 minute. When the pH value reaches 5.5, add 0.1 mol of dopamine hydrochloride. Place the above solution in a reactor and heat to 140°C for 24 hours;

[0100] 3. After the reaction in step 2 is completed, the undried lithium iron phosphate precursor ③ obtained from the reactor is washed clean with 1.0 mol / L ammonia water, and vacuum dried at 110° C. to obtain a dried lithium iron phosphate precursor ③ for standby use;

[0101] 4. Weigh 100 mol of iron phosphate, 52 mol of lithium carbonate, and 10 mol of glucose, mix and dissolve them in deionized water, add 5 mol of the dried lithium iron phosphate precursor ③ obtained in step 3, and then mix the materials with a sand mill and grind them to D 50 ≤400nm. Then, the sand-milled material is spray-dried to form a mixed powder, and the powder is placed in a production line kiln in an inert gas environment and sintered at 780°C for 16 hours, and then cooled and crushed to obtain a carbon-coated lithium iron phosphate finished product③.

[0102] Comparative Example 1

[0103] Weigh 100 mol of iron phosphate, 52 mol of lithium carbonate, and 10 mol of glucose, mix and dissolve them in deionized water, then mix the materials with a sand mill and grind them to D 50 ≤400nm. Then, the sand-milled material is formed into a mixed powder by spray drying, and the powder is placed in a production line kiln in an inert gas environment and sintered at 780°C for 16 hours, and then cooled and crushed to obtain a carbon-coated lithium iron phosphate finished product④.

[0104] Comparative Example 2

[0105] 1. Weigh 10.5 mol of lithium hydroxide, 9.8 mol of ferrous sulfate, and 10 mol of phosphoric acid and dissolve them in 10 L of deionized water respectively. A small amount of green precipitate appears in the mixed solution. Mix the three solutions to obtain a mixed solution ⑤. The pH of the mixed solution is measured to be 3.42;

[0106] 2. Adjust the pH value of the mixed solution ⑤ obtained in step 1 to 4, and then add lithium hydroxide solution to the solution at a rate of 0.01 pH value per minute to slowly increase the pH value to 5.0. Since there is a buffering process in the latter stage of the reaction to avoid the pH value being too high, continue to add lithium hydroxide solution after the pH value is higher than 5.0 and stabilizes for 1 minute. When the pH value reaches 5.5, add 1 mol of dopamine hydrochloride. Place the above solution in a reactor and heat to 140°C for 24 hours;

[0107] 3. After the reaction in step 2 is completed, the undried lithium iron phosphate precursor ⑤ obtained from the reactor is washed clean with 1 mol / L ammonia water, and vacuum dried at 110° C. to obtain a dried lithium iron phosphate precursor ⑤ for standby use;

[0108] 4. Weigh 100 mol of iron phosphate, 52 mol of lithium carbonate, and 10 mol of glucose, mix and dissolve them in deionized water, add 5 mol of the dried lithium iron phosphate precursor ⑤ obtained in step 3, and then mix the materials with a sand mill and grind them to D 50 ≤400nm. Then, the sand-milled material is formed into a mixed powder by spray drying, and the powder is placed in a production line kiln in an inert gas environment and sintered at 780°C for 16 hours, and then cooled and crushed to obtain a carbon-coated lithium iron phosphate finished product⑤.

[0109] Comparative Example 3

[0110] 1. Weigh 5.2 mol of lithium sulfate, 9.8 mol of ferrous sulfate, and 10 mol of phosphoric acid and dissolve them in 10 L of deionized water (the pH value of the solution is lower than 4.0 at this time, and there is no need to add an acidic solution to adjust the pH value). Mix the three solutions to obtain a mixed solution ⑥;

[0111] 2. The pH value of the mixed solution ⑥ obtained in step 1 is quickly adjusted to 4, and the pH value is brought to 5.5 by quickly adding ammonia water. Since the reaction is still going on at this time, the added ammonia water has not completely reacted with the system, and the pH value of the solution will continue to rise. 1 mol of dopamine hydrochloride is added. The above solution is placed in a reactor and heated to 140°C for 24 hours;

[0112] 3. After the reaction in step 2 is completed, the undried lithium iron phosphate precursor ⑥ obtained from the reactor is washed clean with 1 mol / L ammonia water, and vacuum dried at 110° C. to obtain a dried lithium iron phosphate precursor ⑥ for standby use;

[0113] 4. Weigh 100 mol of iron phosphate, 52 mol of lithium carbonate, and 10 mol of glucose, mix and dissolve them in deionized water, add 5 mol of the dried lithium iron phosphate precursor ⑥ obtained in step 3, and then mix the materials with a sand mill and grind them to D 50≤400nm. Then, the sand-milled material is formed into a mixed powder by spray drying, and the powder is placed in a production line kiln in an inert gas environment and sintered at 780°C for 16 hours, and then cooled and crushed to obtain a carbon-coated lithium iron phosphate finished product⑥.

[0114] Comparative Example 4

[0115] 1. Weigh 5.2 mol of lithium sulfate, 9.8 mol of ferrous sulfate, and 10 mol of phosphoric acid and dissolve them in 10 L of deionized water respectively (the pH of the mixed solution is lower than 4.0 at this time, and there is no need to add acidic solution to adjust the pH). Mix the three solutions to obtain a mixed solution ⑦.

[0116] 2. Quickly adjust the pH value of the mixed solution ⑦ obtained in step 1 to 4, and then add lithium hydroxide solution to the solution at a rate of 0.01 pH value per minute to slowly increase the pH value to 5.0. Since there is a buffering process in the latter stage of the reaction to avoid the pH value being too high, lithium hydroxide solution is continued to be added after the pH value is higher than 5.0 and stabilized for 1 minute. When the pH value reaches 5.5, add 1 mol of dopamine hydrochloride. Place the above solution in a reactor and heat to 140°C for 24 hours;

[0117] 3. After the reaction in step 2 is completed, the undried lithium iron phosphate precursor ⑦ obtained from the reactor is washed with deionized water and dried in a vacuum oven at 110° C. to obtain a dried lithium iron phosphate precursor ⑦ for standby use;

[0118] 4. Weigh 100 mol of iron phosphate, 52 mol of lithium carbonate, and 10 mol of glucose, mix and dissolve in deionized water, add 5 mol of the dried lithium iron phosphate precursor ⑦ obtained in step 3, and then mix the materials by a sand mill and crush them to D50≤400nm. Then, spray dry the sand-milled materials to form a mixed powder, place the powder in an inert gas environment in a production line kiln and sinter at 780°C for 16 hours, and cool and crush to obtain a carbon-coated lithium iron phosphate finished product ⑦.

[0119] Comparative Example 5

[0120] 1. Weigh 5.2 mol of lithium sulfate, 9.8 mol of ferrous sulfate, and 10 mol of phosphoric acid and dissolve them in 10 L of deionized water (the pH of the mixed solution is lower than 4.0 at this time, and there is no need to add an acidic solution to adjust the pH), and mix the three solutions to obtain a mixed solution⑧;

[0121] 2. The pH value of the mixed solution ⑧ obtained in step 1 is quickly adjusted to 4, and then lithium hydroxide solution is added to the solution at a rate of 0.01 pH value per minute to slowly increase the pH value to 5.0. Since there is a buffering process in the latter stage of the reaction to avoid excessive pH value, lithium hydroxide solution is continued to be added after the pH value is higher than 5.0 and the pH value is stabilized for 1 minute. When the pH value reaches 5.5, the above solution is placed in a reactor and heated to 140°C for 24 hours;

[0122] 3. After the reaction in step 2 is completed, the undried lithium iron phosphate precursor ⑧ obtained from the reactor is washed clean with 1 mol / L ammonia water, and vacuum dried at 110° C. to obtain a dried lithium iron phosphate precursor ⑧ for standby use;

[0123] 4. Weigh 100 mol of iron phosphate, 52 mol of lithium carbonate, and 10 mol of glucose, mix and dissolve them in deionized water, add 5 mol of the dried lithium iron phosphate precursor⑧ obtained in step 3, and then mix the materials through a sand mill and crush them to D50≤400nm. Then, spray dry the sand-milled materials to form a mixed powder, place the powder in an inert gas environment in a production line kiln and sinter at 780°C for 16 hours, and cool and crush to obtain a carbon-coated lithium iron phosphate finished product⑧.

[0124] Comparative Example 6

[0125] 1. Weigh 5.2 mol of lithium sulfate, 9 mol of ferrous sulfate, and 10 mol of phosphoric acid and dissolve them in 10 L of deionized water (the pH value of the mixed solution is lower than 4.0 at this time, and there is no need to add an acidic solution to adjust the pH value). Mix the three solutions to obtain a mixed solution ⑨;

[0126] 2. Quickly adjust the pH value of the mixed solution ⑨ obtained in step 1 to 4, and then add lithium hydroxide solution to the solution at a rate of 0.01 pH value per minute to slowly increase the pH value to 5.0. Since there is a buffering process in the latter stage of the reaction to avoid the pH value being too high, lithium hydroxide solution is continued to be added after the pH value is higher than 5.0 and stabilized for 1 minute. When the pH value reaches 5.5, add 1 mol of dopamine hydrochloride. Place the above solution in a reactor and heat to 140°C for 24 hours;

[0127] 3. After the reaction in step 2 is completed, the undried lithium iron phosphate precursor ⑨ obtained from the reactor is washed clean with 1 mol / L ammonia water, and vacuum dried at 110° C. to obtain a dried lithium iron phosphate precursor ⑨ for standby use;

[0128] 4. Weigh 100 mol of iron phosphate, 52 mol of lithium carbonate, and 10 mol of glucose, mix and dissolve them in deionized water, add 5 mol of the dried lithium iron phosphate precursor ⑨ obtained in step 3, and then mix the materials through a sand mill and crush them to D50≤400nm. Then, spray dry the sand-milled materials to form a mixed powder, place the powder in an inert gas environment in a production line kiln and sinter at 780°C for 16 hours, and cool and crush to obtain a carbon-coated lithium iron phosphate finished product ⑨.

[0129] Test Case

[0130] A CR2025 button cell was prepared, wherein the positive electrode sheet was composed of the carbon-coated lithium iron phosphate positive electrode materials ① to ⑨ prepared in Examples 1-3 and Comparative Examples 1-6, acetylene black and PVDF (mass ratio of 9:0.5:0.5), and the positive electrode slurry ① to ⑨ was 3 to 4 mg / cm 2 The density of the material was coated on the collector Al foil, and the CR2025 coin-type battery was assembled in an Ar atmosphere glove box. Lithium metal was used as the negative electrode, the electrolyte was 1M LiPF6 solution, and the solvent was a mixed solution of DMC:EMC:EC (volume ratio of 1:1:1). The electrochemical performance of the material was studied using the Xinwei battery test system at different rates (1C=170mAh / g). The variance of the capacity of the sagger at each position was statistically analyzed to analyze the impact of the technical solution on the consistency of the system. The results are shown in the table below.

[0131] Table 1

[0132]

[0133] The results of Examples 1-3 show that the carbon-coated lithium iron phosphate material obtained by the preparation method provided by the present invention has high capacity and good consistency at different sintering positions, which indicates that the preparation method provided by the present invention can effectively improve the electrical performance and consistency of industrially produced carbon-coated lithium iron phosphate materials.

[0134] Comparative Example 1 produces lithium iron phosphate according to the current industrial method without adding a lithium iron phosphate precursor, so the capacity is lower than that of Example 1, and the performance difference between different positions is large, which affects the cycle stability of the material.

[0135] In comparative example 2, when synthesizing the lithium iron phosphate precursor, the soluble lithium source in the raw materials used is lithium hydroxide. Since the lithium hydroxide aqueous solution is strongly alkaline and the pH value of the solution is not adjusted to below 4 before mixing, precipitation occurs when the lithium source, iron source, and phosphorus source are mixed. Although the pH of the mixed solution is lower than 4, the lithium hydroxide solution reacts with other raw materials in advance to form an uneven phase, resulting in the failure of the synthesis of the lithium iron phosphate precursor. Therefore, after adding the synthesized non-target lithium iron phosphate precursor, the capacity is reduced due to the presence of certain inactive substances inside, and its batch consistency cannot be improved.

[0136] In the process of synthesizing the lithium iron phosphate precursor in Comparative Example 3, the ammonia solution was not added slowly when the pH value was adjusted, so that the crystal nuclei could not be formed evenly in the system. The rapid addition of the ammonia solution would lead to local uneven dispersion and the production of non-target intermediates, and the addition of too much ammonia would cause the pH of the mixed solution C to exceed 5.5, and only part of the lithium iron phosphate crystals would be generated. Therefore, the lithium iron phosphate precursor synthesized in Comparative Example 3 has improved consistency compared to Comparative Example 1 in which no lithium iron phosphate precursor was added. However, due to the presence of a large amount of lithium iron phosphate precursor formed by non-lithium iron phosphate crystals, the capacity and consistency of the carbon-coated lithium iron phosphate are lower than those in Example 1.

[0137] In Comparative Example 4, when washing the lithium iron phosphate precursor, ammonia water was not used for washing, resulting in no iron vacancies formed on the surface of the lithium iron phosphate crystals, and the added dopamine hydrochloride was not precipitated. No carbon coating layer was formed on the surface of the lithium iron phosphate crystals, so that no lithium iron phosphate precursor was formed. As a result, when the carbon-coated lithium iron phosphate material was prepared by subsequent high-temperature sintering, its surface composition was consistent with that of industrial lithium iron phosphate, and the particles were melted in the kiln with uneven temperature. Compared with Example 1, its capacity and consistency were poor.

[0138] In Comparative Example 5, dopamine hydrochloride was not added, and no carbon coating layer was formed. Since there was no dopamine hydrochloride protective layer during the washing process, the surface Fe would be excessively complexed, resulting in surface iron deficiency, which led to a decrease in the Fe content of the lithium iron phosphate precursor, and a decrease in the lithium iron phosphate content in the lithium iron phosphate precursor. After high-temperature sintering, due to the Fe deficiency in the lithium iron phosphate precursor, the active material content in the carbon-coated lithium iron phosphate was reduced, resulting in a decrease in capacity and a decrease in heat absorption. The performance gap between different sagger positions was relatively large compared to Example 1, resulting in a decrease in consistency, but it was higher than Comparative Example 1.

[0139] In Comparative Example 6, the proportion of iron added during the synthesis of the lithium iron phosphate precursor is too small. In the washing process, part of the Fe is complexed with ammonia water, resulting in surface iron deficiency, which leads to a decrease in the Fe content of the lithium iron phosphate precursor, and a decrease in the lithium iron phosphate content in the lithium iron phosphate precursor. After high-temperature sintering, due to the Fe deficiency in the lithium iron phosphate precursor, the content of the carbon-coated lithium iron phosphate active material is reduced, resulting in a decrease in capacity and a decrease in heat absorption. Compared with Example 1, the performance gap between different sagger positions is large, resulting in a decrease in consistency but higher than that of Comparative Example 1.

[0140] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0141] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a lithium iron phosphate precursor, characterized in that: include: preparing a first lithium source solution, a first iron source solution, and a first phosphorus source solution, and adjusting the pH values ​​of the first lithium source solution, the first iron source solution, and the first phosphorus source solution to be less than 4.0; Mixing the first lithium source solution, the first iron source solution, and the first phosphorus source solution to obtain a mixed solution a; Adjusting the pH value of the mixed solution a until a precipitate is generated in the mixed solution a to obtain a mixed solution b; Controlling the pH value of the mixed solution b to increase by 0.01-0.1 per minute, adjusting the pH value of the mixed solution b to 5.0-5.5, to obtain a mixed solution c; Adding a first carbon source to the mixed solution c for liquid phase reaction to obtain lithium iron phosphate crystals; The lithium iron phosphate crystals are washed with a weak alkaline solution to obtain the lithium iron phosphate precursor.

2. The preparation method according to claim 1, characterized in that: The first lithium source in the first lithium source solution includes at least one selected from the group consisting of lithium sulfate, lithium acetate, lithium nitrate, lithium gluconate, lithium chloride, lithium hydroxide, and lithium fluoride; Optionally, the first iron source in the first iron source solution includes at least one selected from ferrous sulfate, ferric nitrate, ferric gluconate, ferrous chloride, and ferric fluoride; Optionally, the first phosphorus source in the first phosphorus source solution includes at least one selected from phosphoric acid, ammonium monohydrogen phosphate, and ammonium dihydrogen phosphate; Optionally, the first lithium source solution, the first iron source solution, and the first phosphorus source solution are mixed according to an element molar ratio of Li:Fe:P of (1.0-1.05):(0.95-1):

1.

3. The preparation method according to claim 1, characterized in that: The first carbon source comprises at least one selected from dopamine hydrochloride, glucose, gluconolactone, and polyethylene glycol; Among them, at least dopamine hydrochloride is included.

4. The preparation method according to claim 1, characterized in that: The molar ratio of the first carbon source to the first phosphorus source is (0.01-0.2):

1.

5. The preparation method according to claim 1, characterized in that: The liquid phase reaction temperature is 80-180°C; Optionally, the liquid phase reaction time is 8-36 hours.

6. The preparation method according to claim 1, characterized in that: The weak alkaline solution is at least one of an ammonia solution, an ethylenediamine solution, a triethanolamine solution, an aniline solution, and an alkyl alcoholamine solution; The molar concentration of the weakly alkaline solution is 0.1-2 mol / L.

7. A lithium iron phosphate precursor, characterized in that: The lithium iron phosphate precursor is obtained according to the preparation method according to any one of claims 1-6.

8. A method for preparing carbon-coated lithium iron phosphate, characterized in that: include: Mixing a lithium iron phosphate precursor with a second lithium source, a second iron source, a second phosphorus source, and a second carbon source, and sintering to obtain the carbon-coated lithium iron phosphate; Wherein, the lithium iron phosphate precursor is obtained according to the preparation method according to any one of claims 1 to 6 or is the lithium iron phosphate precursor according to claim 7.

9. The preparation method according to claim 8, characterized in that: The second lithium source includes at least one selected from lithium carbonate, lithium phosphate, and lithium oxalate; Optionally, the second iron source includes at least one selected from ferric phosphate, ferrous phosphate, ferric oxide, and ferrous oxalate; Optionally, the second phosphorus source includes at least one selected from iron phosphate, ammonium dihydrogen phosphate, and lithium hydrogen phosphate; Optionally, the second carbon source comprises at least one selected from glucose, ethylene glycol, toluene, n-octane, and ethyl acetate; Optionally, the second lithium source, the second iron source, and the second phosphorus source are mixed according to an element molar ratio of Li:Fe:P of (1-1.05):1:(1-1.05); Optionally, the molar ratio of the lithium iron phosphate precursor to the iron element in the second lithium source, the second iron source, the second phosphorus source, and the second carbon source is 0.01 to 0.1:1; Optionally, the molar ratio of the second carbon source to the lithium iron phosphate precursor is 1 to 10:

1.

10. A carbon-coated lithium iron phosphate, characterized in that: The carbon-coated lithium iron phosphate is obtained according to the preparation method of claim 8 or 9.

Citation Information

Patent Citations

  • Novel green lithium iron phosphate precursor as well as preparation method and application thereof

    CN113896182A

  • Method for preparing carbon-coated modified lithium iron phosphate positive electrode

    CN117088348A

  • Preparation method of carbon-coated lithium iron phosphate

    CN117317183A

  • Method for recovering and preparing lithium iron phosphate cathode material

    WO2020134773A1

  • Iron phosphate precursor and preparation method therefor and application thereof

    WO2022227669A1