Normal-pressure preparation method of high-transmittance hydrophobic silicon-based bulk aerogel
By using acid catalysts and surfactants to treat silicon-based sols under normal pressure, the complexity and high cost of traditional drying processes are solved, and a high-transparent hydrophobic silicon-based block aerogel is prepared, achieving low cost and safety The material preparation meets the thermal insulation and light transmission needs of building glass.
Patent Information
- Application Number
- CN202411098503.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-12
AI Technical Summary
Traditional supercritical drying processes are complex, the equipment costs are high, the high temperature and high pressure operation is very dangerous, and normal pressure drying causes gel shrinkage and cracking, making it difficult to ensure light transmittance.
The aqueous acid catalyst solution reacts with the precursor containing organic groups to form a silicon-based sol, and the pH is adjusted by adding surfactant and alkali catalyst to form a wet gel with a complete structure and dried under normal pressure through multiple solvent replacement and natural evaporation. , a high light-transmitting hydrophobic silicon-based block aerogel was obtained.
Overcoming the complexity and high cost of supercritical drying, it realizes the preparation of high-light translucent hydrophobic silicon-based block aerogel with simple operation and safe green operation, with a thermal conductivity of 0.025 W/(m·K), and a high light transmittance. Good hydrophobic properties and are suitable for architectural glass applications.
Smart Images

Figure CN118877902A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanoporous aerogel material preparation, and in particular to a method for preparing a highly light-transmitting hydrophobic silicon-based block aerogel at normal pressure. Background Art
[0002] In recent years, there have been a large number of literature reports and patent disclosures related to block silicon-based aerogel materials and their preparation processes. However, problems related to the atmospheric pressure preparation of transparent block silicon-based aerogel materials and their engineering applications have also arisen. The maintenance of the integrity of the material block structure is highly dependent on the drying method of the gel. Supercritical drying is used to reduce or even eliminate the capillary tension of the solvent in the pores of the wet gel. However, due to factors such as high equipment cost, complex process, and long drying time, the further development and industrial application of supercritical drying in aerogel preparation are limited.
[0003] The publication number is CN105271263A, and the invention name is a patent for a low-density transparent silica aerogel and its preparation method. The silica gel is prepared by mixing water, alcohol, and hexamethyldisiloxane, adding them to a reactor for heating reaction, and further catalyzing them with hydrofluoric acid. The aerogel obtained after supercritical drying has a thermal conductivity (25°C) of at least 0.012W / (m·K) and good transparency. The publication number is CN117699808A, and the invention name is a patent for a method for preparing a highly efficient and heat-insulating lightweight transparent silica aerogel material. The aerogel obtained after supercritical drying has a thermal conductivity of at least 0.010W / (m·K) at room temperature and good transmittance. However, the preparation process of the above-mentioned transparent block aerogel is relatively complicated, and more drugs are used. The supercritical drying method of carbon dioxide is complicated, the equipment cost is high, and the high temperature and high pressure operation is dangerous.
[0004] Although the preparation of aerogel by normal pressure drying is simple, low-cost, safe and green, it does not eliminate the influence of capillary pressure during solvent evaporation, so the shrinkage and cracking of the gel during the drying process are difficult to avoid, and it is difficult to ensure its light transmittance. Therefore, it is necessary to improve it to ensure the integrity of the material and enhance the relevant properties of the material. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing highly transparent hydrophobic silicon-based block aerogel at normal pressure, which solves the technical problems of complex traditional supercritical drying process, high equipment cost, and high risk of high temperature and high pressure operation.
[0006] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a highly light-transmitting hydrophobic silicon-based block aerogel under normal pressure, the normal pressure preparation method comprising the following steps: S1, preparing an acid catalyst aqueous solution, and adding a precursor containing an organic group to the acid catalyst aqueous solution to obtain a completely hydrolyzed silica-based sol after mixing evenly; S2, adding surfactant and deionized water to the silica-based sol and mixing evenly, adjusting the pH of the silica-based sol to 8-9, and letting it stand to form a gel after metering and aging to obtain a silica-based wet gel with a complete structure; S3, soaking the silicon-based wet gel in the replacement solution for multiple times, and regularly replacing the replacement solvent with different concentrations to obtain a block wet gel with complete solvent replacement; S4. The wet block gel is placed under normal pressure at different temperature gradients and maintained for a corresponding period of time, so that the liquid in the gel pores evaporates completely, thereby obtaining a completely dried, highly transparent, hydrophobic silicon-based block aerogel.
[0007] Furthermore, in step S1, the specific process includes: Mix deionized water and an acid catalyst in proportion to obtain an acid catalyst aqueous solution with a concentration of 5 to 20 mmol / L; A precursor with an unhydrolyzable organic group is added to an acid catalyst aqueous solution, and a magnetic stirrer is used to stir the precursor to form a completely hydrolyzed silica-based sol. The stirring temperature, speed and time are 20-30° C., 400-600 r / min and 30-60 min, respectively.
[0008] Furthermore, the acid catalyst includes but is not limited to any one of acetic acid, hydrochloric acid, oxalic acid, sulfuric acid, nitric acid, phosphoric acid or citric acid.
[0009] Furthermore, the mass ratio of the acid catalyst aqueous solution to the precursor containing organic groups is 5:5-6:4, and the amount of the acid catalyst added is to adjust the pH of the silica-based sol to 5-6.
[0010] Furthermore, the precursor containing an organic group is an organic substance of R1-Si-(OR2)3, wherein R1 and R2 represent alkyl groups respectively, including but not limited to any one of methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), and ethyltriethoxysilane (ETMS).
[0011] Furthermore, in step S2, the specific process includes: Adding surfactant and deionized water to the silica-based sol, adjusting the speed of the magnetic stirrer, and continuously stirring the silica-based sol until it becomes uniform, wherein the mass of the surfactant is 20% to 30% of the mass of the precursor containing the organic group, and the mass ratio of deionized water to the surfactant is 8:2 to 7:3; Then, a 0.25-0.5 mol / L aqueous solution of a base catalyst is added to the stirred silica-based sol and stirred to make the pH of the silica-based sol 8-9; Finally, the silica-based sol with a pH of 8 to 9 is transferred to a customized mold, allowed to stand to form a gel and then demolded after aging to obtain a structurally complete silica-based wet gel, and the integrity of the gel block structure is ensured during the demolding process.
[0012] Further, the surfactant includes but is not limited to any one of cetyltrimethylammonium chloride (CTAB), cetyltrimethylammonium bromide (CTAC), polyoxyethylene polyoxypropylene (F127), and poloxamer 188 (F68); The alkaline catalyst aqueous solution is a mixed solution of deionized water and an alkaline catalyst, and the alkaline catalyst includes but is not limited to any one of ammonia water, urea, NaOH, KOH, tetramethylammonium hydroxide (TMAOH), and tetraethylammonium hydroxide (TEAOH).
[0013] Furthermore, the temperature, rotation speed and duration of the mixing and stirring are 0-15°C, 100-250 r / min and 30-60 min respectively.
[0014] Furthermore, in step S3, the specific process includes: Prepare a replacement solution with a volume of 5 to 8 times the volume of the gel, the replacement solution is divided into ethanol aqueous solution and n-hexane aqueous solution of different concentrations, the ethanol aqueous solution of different concentrations is deionized water: ethanol volume ratio = 100:0, 70:30, 50:50, 30:70, 0:100; The silicon-based wet gel is soaked in ethanol aqueous solutions of different concentrations once, and then repeatedly soaked in n-hexane aqueous solution for 3 times to obtain a block wet gel with complete solvent replacement. The temperature of the replacement solution is controlled at 26-40°C, and the soaking time is at least 8 hours each time.
[0015] Further, in step S4, different temperature gradients are maintained at normal pressure for corresponding time, specifically: The temperature and duration of the first drying are 25-40°C and 2-4h respectively; the temperature and duration of the second drying are 60-80°C and 3-5h respectively; the temperature and duration of the final drying are 100-120°C and 4-6h respectively.
[0016] By means of the above technical solution, the present invention provides a method for preparing highly transparent hydrophobic silicon-based block aerogel at normal pressure, which has at least the following beneficial effects: 1. The present invention overcomes the shortcomings of supercritical drying, which has complex process, high equipment cost, and high risk of high temperature and high pressure operation. Block silicon-based aerogel is prepared by natural evaporation and normal pressure drying. The obtained aerogel has excellent hydrophobicity and high light transmittance, and the thermal conductivity (room temperature environment) is 0.025 W / (m·K).
[0017] 2. The present invention uses MTMS as a precursor containing an organic group, and does not require subsequent hydrophobic modification and modification processes, thereby simplifying the preparation steps. The aerogel obtained has good hydrophobicity and a contact angle of >90°, and is a hydrophobic material.
[0018] 3. The surfactant F127 of the present invention is a triblock structure of polyethylene oxide-polypropylene oxide, forming a symmetrical structure of PEO-PPO-PEO, which makes it "amphiphilic" and can interact with hydrophobic surfaces and biomembranes, moderately inhibit macroscopic phase separation, determine the gel skeleton structure, and thus produce a silicon-based aerogel with higher light transmittance.
[0019] 4. The present invention uses TMAOH as an alkaline catalyst. Compared with other alkaline catalysts, TMAOH can quickly increase the pH of the sol to the required value with a very small amount, saving reagents in the preparation process and reducing the gel formation time; and TMAOH can more effectively inhibit the phase separation trend. The prepared aerogel has a higher transmittance, a wavelength range of 600-800nm, and a light transmittance of >80%. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings: Figure 1 This is a macroscopic morphology of a highly transparent hydrophobic silicon-based bulk aerogel material prepared at normal pressure in the present invention; Figure 2 This is a microscopic morphology of a highly transparent hydrophobic silicon-based bulk aerogel material prepared at normal pressure in the present invention; Figure 3 Schematic diagram of the hydrophobic angle of the highly transparent hydrophobic silicon-based bulk aerogel material prepared at normal pressure of the present invention; Figure 4 Schematic diagram of visible light transmittance of highly transparent hydrophobic silicon-based block aerogel material prepared at normal pressure in the present invention. DETAILED DESCRIPTION
[0021] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific implementation methods, so that the implementation process of how the present application uses technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.
[0022] According to the heat transfer mechanism of architectural glass, the main factors affecting its energy consumption are its own thermal conductivity and radiation transmittance. At present, technologies including vacuum, coating, and multi-layer insulating glass have been used to improve its thermal insulation capacity. However, in subsequent studies, it is not difficult to find that the preparation conditions of vacuum and multi-layer insulating glass are relatively high and the structure is complex; coated glass has little effect on infrared light from solar radiation and has a low radiation transmittance. Therefore, some scholars use materials with extremely low thermal conductivity and high radiation transmittance to fill the glass interlayer, which can effectively improve the thermal insulation capacity of architectural glass. Among them, aerogel has become an ideal choice for architectural glass composite materials due to its low density, high porosity, low thermal conductivity, low refractive index and high light transmittance.
[0023] In recent years, there have been a large number of literature reports and patent disclosures on block silicon-based aerogel materials and their preparation processes, but the problems caused by the atmospheric pressure preparation of transparent block silicon-based aerogel materials and their engineering applications have also followed. The maintenance of the integrity of the material block structure is highly dependent on the drying method of the gel. Supercritical drying is used to reduce or even eliminate the capillary tension of the solvent in the pores of the wet gel, but due to its high equipment cost, complex process, long drying time and other factors, the further development and industrial application of supercritical drying in aerogel preparation are limited. In addition, although the preparation of aerogel by atmospheric pressure drying is simple, low-cost, safe and green, it is difficult to avoid the shrinkage and cracking of the gel during the drying process, and it is difficult to ensure its transmittance, because it does not eliminate the influence of the capillary pressure during solvent evaporation. Therefore, the traditional preparation process is relatively complicated and uses more drugs. The supercritical drying method of carbon dioxide is complex, the equipment cost is high, and the high temperature and high pressure operation is dangerous. Therefore, it is necessary to improve it to ensure the integrity of the material and improve the relevant properties of the material.
[0024] In order to realize a silicon-based bulk aerogel material with a certain transmittance under normal pressure and drying conditions, and to improve its transmittance and integrity as much as possible while ensuring its low thermal conductivity to meet the application requirements of architectural glass, this embodiment proposes a normal pressure preparation method for highly transmittance hydrophobic silicon-based bulk aerogel, and it is achieved through the preparation methods proposed in Examples 1 to 4.
[0025] Among them, methyltrimethoxysilane (MTMS) is used as a precursor containing an organic group; acetic acid is used as an acid catalyst, and a tetramethylammonium hydroxide (TMAOH) aqueous solution is used as a base catalyst, and its mass is 2% to 9% of the mass of methyltrimethoxysilane (MTMS). Methyltrimethoxysilane (MTMS) undergoes hydrolysis and polycondensation under the catalysis of acetic acid and tetramethylammonium hydroxide (TMAOH), which can regulate the prepolymerization degree and skeleton structure of the primary and secondary particles of silica; polyoxyethylene polyoxypropylene (F127) is used as a surfactant, and ethanol and n-hexane are preferably used as solvent replacement reagents. Their non-water solubility and low surface tension characteristics are beneficial to phase separation and polycondensation reactions, so that high-transmittance hydrophobic silicon-based block aerogel can be prepared by drying at normal pressure. Example 1
[0026] A method for preparing a highly transparent hydrophobic silicon-based block aerogel at normal pressure according to Example 1 of the present invention comprises the following steps: Step 1: Preparation of silica-based sol: deionized water and acetic acid are mixed to obtain a 5 mmol / L acetic acid aqueous solution; 10 parts of the acetic acid aqueous solution and 10 parts of methyltrimethoxysilane (MTMS) are mixed, the pH of the silica-based sol is adjusted to 5-6, and a magnetic stirrer is used to stir to fully hydrolyze methyltrimethoxysilane (MTMS) to form a completely hydrolyzed silica-based sol, the rotation speed is 500 rpm / min, and the stirring temperature and time are 25°C and 20 minutes respectively; Step 2: Formation and aging of silicon-based wet gel: 2 parts of surfactant polyoxyethylene polyoxypropylene (F127) and 8 parts of deionized water are added to the silicon-based sol formed in step 1 and mixed, and stirred with a magnetic stirrer to make the mixture uniform, the speed is 300 rpm / min, and the stirring temperature and time are 10°C and 20 minutes respectively; Deionized water and tetramethylammonium hydroxide (TMAOH) are mixed to obtain a 0.25 mol / L TMAOH aqueous solution; 0.5 parts of the TMAOH aqueous solution are added to the above uniform silica-based sol to adjust the pH of the silica-based sol to 8-9, the obtained silica-based sol is transferred to a customized mold, and allowed to stand until the gel is completely formed, and then the gel is demolded, and the integrity of the gel block structure is ensured during the demolding process to obtain a complete block of silica-based wet gel; Step 3: Solvent replacement: The silicon-based wet gel prepared in step 2 was immersed in the replacement solvent for multiple times, the volume of the replacement solvent was 8 times the volume of the silicon-based wet gel, and the composition of the replacement solvent was changed in the following order: deionized water: ethanol volume ratio = 100:0, 70:30, 50:50, 30:70, 0:100, n-hexane; wherein, the ethanol-water solution was immersed once at each concentration, and the n-hexane solution was immersed 3 times, and the solvent was replaced every 12 hours to obtain a block wet gel with complete solvent exchange, and the replacement temperature was 30°C; Step 4: Formation of aerogel: The block wet gel obtained in step 3 is treated by natural evaporation and normal pressure drying. The temperature and duration of the initial drying are 25-40°C and 3h, respectively; the temperature and duration of the second drying are 60°C and 4h, respectively; the temperature and duration of the final drying are 100°C and 4h, respectively; a highly transparent hydrophobic silicon-based block aerogel is obtained. Example 2
[0027] A method for preparing a highly transparent hydrophobic silicon-based block aerogel at normal pressure according to Example 2 of the present invention comprises the following steps: Step 1: Preparation of silica-based sol: deionized water and acetic acid are mixed to obtain a 5 mmol / L acetic acid aqueous solution; 12 parts of the acetic acid aqueous solution and 8 parts of methyltrimethoxysilane (MTMS) are mixed, the pH of the silica-based sol is adjusted to 5-6, and a magnetic stirrer is used to stir to fully hydrolyze methyltrimethoxysilane (MTMS) to form a completely hydrolyzed silica-based sol, the rotation speed is 500 rpm / min, and the stirring temperature and time are 25°C and 20 minutes respectively; Step 2: Formation and aging of silicon-based wet gel: 3 parts of surfactant polyoxyethylene polyoxypropylene (F127) and 8 parts of deionized water are added to the silicon-based sol formed in step 1 and mixed, and stirred with a magnetic stirrer to make the mixture uniform, the speed is 300 rpm / min, and the stirring temperature and time are 10°C and 20 minutes respectively; Deionized water and tetramethylammonium hydroxide (TMAOH) are mixed to obtain a 0.25 mol / L TMAOH aqueous solution; 0.75 parts of the TMAOH aqueous solution are added to the above uniform silica-based sol to adjust the pH of the silica-based sol to 8-9, the obtained silica-based sol is transferred to a customized mold, and allowed to stand until the gel is completely formed, and then the gel is demolded, and the integrity of the gel block structure is ensured during the demolding process to obtain a complete block of silica-based wet gel; Step 3: Solvent replacement: The silicon-based wet gel prepared in step 2 was immersed in the replacement solvent for multiple times, the volume of the replacement solvent was 8 times the volume of the silicon-based wet gel, and the composition of the replacement solvent was changed in the following order: deionized water: ethanol volume ratio = 100:0, 70:30, 50:50, 30:70, 0:100, n-hexane; wherein, the ethanol-water solution was immersed once at each concentration, and the n-hexane solution was immersed 3 times, and the solvent was replaced every 12 hours to obtain a block wet gel with complete solvent exchange, and the replacement temperature was 30°C; Step 4: Formation of aerogel: The block wet gel obtained in step 3 is treated by natural evaporation and normal pressure drying. The temperature and duration of the initial drying are 25-40°C and 3h, respectively; the temperature and duration of the second drying are 60°C and 4h, respectively; the temperature and duration of the final drying are 100°C and 4h, respectively; a highly transparent hydrophobic silicon-based block aerogel is obtained. Example 3
[0028] A method for preparing a highly light-transmitting hydrophobic silicon-based block aerogel at normal pressure according to Example 3 of the present invention comprises the following steps: Step 1: Preparation of silica-based sol: deionized water and acetic acid are mixed to obtain a 5 mmol / L acetic acid aqueous solution; 13 parts of the acetic acid aqueous solution and 7 parts of methyltrimethoxysilane (MTMS) are mixed, the pH of the silica-based sol is adjusted to 5-6, and a magnetic stirrer is used to stir to fully hydrolyze methyltrimethoxysilane (MTMS) to form a completely hydrolyzed silica-based sol, the rotation speed is 500 rpm / min, and the stirring temperature and time are 25°C and 20 minutes respectively; Step 2: Formation and aging of silicon-based wet gel: 2.5 parts of polyoxyethylene polyoxypropylene (F127) and 8 parts of deionized water were added to the silicon-based sol formed in step 1 and mixed, and stirred with a magnetic stirrer to make the mixture uniform, the speed was 300 rpm / min, and the stirring temperature and time were 10°C and 20 min respectively; Deionized water and tetramethylammonium hydroxide (TMAOH) are mixed to obtain a 0.25 mol / L TMAOH aqueous solution; 1 part of the TMAOH aqueous solution is added to the above-mentioned silica-based sol to adjust the pH of the silica-based sol to 8-9, the obtained silica-based sol is transferred to a customized mold, and allowed to stand until the gel is completely formed, and then the gel is demolded, and the integrity of the gel block structure is ensured during the demolding process to obtain a complete block of silica-based wet gel; Step 3: Solvent replacement: The silicon-based wet gel prepared in step 2 was immersed in the replacement solvent for multiple times, the volume of the replacement solvent was 8 times the volume of the silicon-based wet gel, and the composition of the replacement solvent was changed in the following order: deionized water: ethanol volume ratio = 100:0, 70:30, 50:50, 30:70, 0:100, n-hexane; wherein, the ethanol-water solution was immersed once at each concentration, and the n-hexane solution was immersed 3 times, and the solvent was replaced every 12 hours to obtain a block wet gel with complete solvent exchange, and the replacement temperature was 30°C; Step 4: Formation of aerogel: The block wet gel obtained in step 3 is treated by natural evaporation and normal pressure drying. The temperature and duration of the initial drying are 25-40°C and 3h, respectively; the temperature and duration of the second drying are 60°C and 4h, respectively; the temperature and duration of the final drying are 100°C and 4h, respectively; a highly transparent hydrophobic silicon-based block aerogel is obtained. Example 4
[0029] A method for preparing a highly light-transmitting hydrophobic silicon-based block aerogel at normal pressure according to Example 4 of the present invention comprises the following steps: Step 1: Preparation of silica-based sol: deionized water and acetic acid are mixed to obtain a 5 mmol / L acetic acid aqueous solution; 14 parts of the acetic acid aqueous solution and 6 parts of methyltrimethoxysilane (MTMS) are mixed, the pH of the silica-based sol is adjusted to 5-6, and a magnetic stirrer is used to stir to fully hydrolyze methyltrimethoxysilane (MTMS) to form a completely hydrolyzed silica-based sol, the rotation speed is 500 rpm / min, and the stirring temperature and time are 25°C and 20 minutes respectively; Step 2: Formation and aging of silicon-based wet gel: 2.5 parts of polyoxyethylene polyoxypropylene (F127) and 8 parts of deionized water were added to the silicon-based sol formed in step 1 and mixed, and stirred with a magnetic stirrer to make the mixture uniform, the speed was 300 rpm / min, and the stirring temperature and time were 10°C and 20 min respectively; Deionized water and tetramethylammonium hydroxide (TMAOH) are mixed to obtain a 0.25 mol / L TMAOH aqueous solution; 1.25 parts of the TMAOH aqueous solution are added to the above uniform silica-based sol to adjust the pH of the silica-based sol to 8-9, the obtained silica-based sol is transferred to a customized mold, and allowed to stand until the gel is completely formed, and then the gel is demolded, and the integrity of the gel block structure is ensured during the demolding process to obtain a complete block of silica-based wet gel; Step 3: Solvent replacement: The silicon-based wet gel prepared in step 2 was immersed in the replacement solvent for multiple times, the volume of the replacement solvent was 8 times the volume of the silicon-based wet gel, and the composition of the replacement solvent was changed in the following order: deionized water: ethanol volume ratio = 100:0, 70:30, 50:50, 30:70, 0:100, n-hexane; wherein, the ethanol-water solution was immersed once at each concentration, and the n-hexane solution was immersed 3 times, and the solvent was replaced every 12 hours to obtain a block wet gel with complete solvent exchange, and the replacement temperature was 30°C; Step 4: Formation of aerogel: The block wet gel obtained in step 3 is treated by natural evaporation and normal pressure drying. The temperature and duration of the initial drying are 25-40°C and 3h, respectively; the temperature and duration of the secondary drying are 60°C and 4h, respectively; the temperature and duration of the final drying are 100°C and 4h, respectively; a highly transparent hydrophobic silicon-based block aerogel is obtained.
[0030] Verification example: The highly transparent hydrophobic silicon-based bulk aerogel materials prepared by Examples 1 to 4 of the present invention have macroscopic morphology, microscopic morphology, hydrophobic angle schematic diagram, and visible light transmittance schematic diagram as shown in FIG. Figure 1-Figure 4 As shown, in Figure 1 The figure shows the light transmittance of the obtained aerogel. The aerogel background is placed under the real object. The properties of the flexible composite phase change material of each embodiment are shown in Table 1. Figure 1-Figure 4 As shown in Table 1, the specific surface area of the present invention is greater than 550m² / g, the thermal conductivity (room temperature environment) is lower than 0.025 W / (m·K), the transmittance in the visible light band (600-800nm) is greater than 75%, and the hydrophobic angle is greater than 100°. Under normal pressure preparation conditions, the prepared material meets the characteristics of silicon-based block aerogel materials, has relatively ideal hydrophobic, heat-insulating and light-transmitting effects, and the preparation process is simple to operate, low in cost, safe and green, and meets the characteristics of architectural glass filling materials.
[0031] Table 1 Performance of highly transparent hydrophobic silicon-based bulk aerogels in various examples
[0032] Compared with the supercritical drying process, the atmospheric pressure preparation method proposed in the present invention saves reagents in the preparation process, reduces the preparation time, is simple to operate, low in cost, safe and green, and can be dried under atmospheric pressure to prepare a highly transmittance hydrophobic silicon-based block aerogel with a thermal conductivity (room temperature environment) of 0.025 W / (m·K). While ensuring its low thermal conductivity, its transmittance and integrity are improved as much as possible, which can meet the application requirements of architectural glass.
[0033] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0034] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a highly transparent hydrophobic silicon-based bulk aerogel at normal pressure, characterized in that: The normal pressure preparation method comprises the following steps: S1, preparing an acid catalyst aqueous solution, and adding a precursor containing an organic group to the acid catalyst aqueous solution to obtain a completely hydrolyzed silica-based sol after mixing evenly; S2, adding surfactant and deionized water to the silica-based sol and mixing evenly, adjusting the pH of the silica-based sol to 8-9, and letting it stand to form a gel after metering and aging to obtain a silica-based wet gel with a complete structure; S3, soaking the silicon-based wet gel in the replacement solution for multiple times, and regularly replacing the replacement solvent with different concentrations to obtain a block wet gel with complete solvent replacement; S4. The wet block gel is placed under normal pressure at different temperature gradients and maintained for a corresponding period of time, so that the liquid in the gel pores evaporates completely, thereby obtaining a completely dried, highly transparent, hydrophobic silicon-based block aerogel.
2. The normal pressure preparation method according to claim 1, characterized in that: In step S1, the specific process includes: Mix deionized water and an acid catalyst in proportion to obtain an acid catalyst aqueous solution with a concentration of 5 to 20 mmol / L; A precursor with an unhydrolyzable organic group is added to an acid catalyst aqueous solution, and a magnetic stirrer is used to stir the precursor to form a completely hydrolyzed silica-based sol. The stirring temperature, speed and time are 20-30° C., 400-600 r / min and 30-60 min, respectively.
3. The normal pressure preparation method according to claim 1 or 2, characterized in that: The acid catalyst includes, but is not limited to, any one of acetic acid, hydrochloric acid, oxalic acid, sulfuric acid, nitric acid, phosphoric acid or citric acid.
4. The normal pressure preparation method according to claim 1 or 2, characterized in that: The mass ratio of the acid catalyst aqueous solution to the precursor containing organic groups is 5:5-6:4, and the amount of the acid catalyst added is to adjust the pH of the silicon-based sol to 5-6.
5. The normal pressure preparation method according to claim 1 or 2, characterized in that: The precursor containing an organic group is an organic substance of R1-Si-(OR2)3, wherein R1 and R2 represent alkyl groups respectively, including but not limited to any one of methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), and ethyltriethoxysilane (ETMS).
6. The normal pressure preparation method according to claim 1, characterized in that: In step S2, the specific process includes: Adding surfactant and deionized water to the silica-based sol, adjusting the speed of the magnetic stirrer, and continuously stirring the silica-based sol until it becomes uniform, wherein the mass of the surfactant is 20% to 30% of the mass of the precursor containing the organic group, and the mass ratio of deionized water to the surfactant is 8:2 to 7:3; Then, a 0.25-0.5 mol / L aqueous solution of a base catalyst is added to the stirred silica-based sol and stirred to make the pH of the silica-based sol 8-9; Finally, the silica-based sol with a pH of 8 to 9 is transferred to a custom mold, allowed to stand to form a gel, and after aging, the gel is demoulded to obtain a silica-based wet gel with a complete structure.
7. The normal pressure preparation method according to claim 1 or 6, characterized in that: The surfactant includes but is not limited to any one of cetyltrimethylammonium chloride (CTAB), cetyltrimethylammonium bromide (CTAC), polyoxyethylene polyoxypropylene (F127), and poloxamer 188 (F68); The alkaline catalyst aqueous solution is a mixed solution of deionized water and an alkaline catalyst, and the alkaline catalyst includes but is not limited to any one of ammonia water, urea, NaOH, KOH, tetramethylammonium hydroxide (TMAOH), and tetraethylammonium hydroxide (TEAOH).
8. The normal pressure preparation method according to claim 6, characterized in that: The temperature, rotation speed and duration of the mixing and stirring are 0-15°C, 100-250 r / min and 30-60 min respectively.
9. The normal pressure preparation method according to claim 1, characterized in that: In step S3, the specific process includes: Prepare a replacement solution with a volume of 5 to 8 times the volume of the gel, the replacement solution is divided into ethanol aqueous solution and n-hexane aqueous solution of different concentrations, the ethanol aqueous solution of different concentrations is deionized water: ethanol volume ratio = 100:0, 70:30, 50:50, 30:70, 0:100; The silicon-based wet gel is soaked in ethanol aqueous solutions of different concentrations once, and then repeatedly soaked in n-hexane aqueous solution for 3 times to obtain a block wet gel with complete solvent replacement. The temperature of the replacement solution is controlled at 26-40°C, and the soaking time is at least 8 hours each time.
10. The normal pressure preparation method according to claim 1, characterized in that: In step S4, different temperature gradients are maintained at normal pressure for corresponding time periods, specifically: The temperature and duration of the first drying are 25-40°C and 2-4h respectively; the temperature and duration of the second drying are 60-80°C and 3-5h respectively; the temperature and duration of the final drying are 100-120°C and 4-6h respectively.
Citation Information
Patent Citations
Method for preparing wave-transmission SiO2 aerogel heat-insulation composite material by using normal-pressure drying equipment
CN102531521A
Ultralow-density transparent silicon dioxide aerogel capable of being post-cleaned as well as preparation method and application of ultralow-density transparent silicon dioxide aerogel
CN112299428A
Preparation method of transparent hydrophobic aerogel
CN112320808A
Wave-transmitting, efficient and heat-insulating aerogel composite material and preparation method thereof
CN112851292A
Method for preparing hydrophobic SiO2 aerogel material through normal-pressure drying
CN113353942A
Cited By
A modified MTES-based transparent silica aerogel and a preparation method thereof
CN122725287A