Method for producing white carbon black from fluorine-containing silicon slag, white carbon black and application of white carbon black

By reacting sodium carbonate with sodium hydroxide with fluorinated silicone slag, and adding surfactant and CO2 gas, the problem of fluorinated silicone slag treatment in the fluorinated silicone slag method is solved, and the dispersion and fluidity of white carbon black is improved. , achieving high-efficiency fluorine and silicon yields and environmentally friendly production process.

CN118877903AActive Publication Date: 2024-11-01GUIZHOU WENGFU LANTIAN FLUORCHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410909918.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively treat fluorinated silicon slag produced in the process of producing anhydrous hydrogen fluoride by fluorosilicate, resulting in insufficient dispersion and fluidity of white carbon black products, and poor economic benefits.

Method used

Sodium carbonate and sodium hydroxide and fluorinated silicone slag are reacted to form a mixed solution of sodium fluorinated sodium silicate, and surfactant and CO2 gas are added, solid-liquid separation and washing are performed, followed by drying with n-butanol to increase the white carbon black dispersibility and liquidity.

Benefits of technology

The yield of high-efficiency fluorine and silicon is achieved, and the obtained white carbon black products have excellent dispersion and fluidity, meet the strict requirements of high-end application fields, and reduce environmental pollution and wastewater generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877903A_ABST
    Figure CN118877903A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fluorine-containing silicon slag recycling, in particular to a method for producing white carbon black from fluorine-containing silicon slag, the white carbon black and application of the white carbon black. The method comprises the following steps: S1, mixing sodium carbonate and sodium hydroxide, reacting the mixture with fluorine-containing silicon slag to obtain a fluorine-containing sodium silicate mixed solution, and adding a surfactant into the fluorine-containing sodium silicate mixed solution; and S2, introducing CO2 gas into the sodium fluosilicate-containing mixed solution added with the surfactant to react, carrying out solid-liquid separation on the reactant, washing the obtained solid phase, adding n-butyl alcohol, uniformly mixing, and drying to obtain the sodium fluosilicate-containing composite material. According to the production method disclosed by the invention, the fluorosilicone yield in the process of preparing the white carbon black is high, and the obtained white carbon black product is excellent in quality and good in dispersity and flowability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of recycling fluorine-containing silicon slag, and in particular to a method for producing white carbon black from fluorine-containing silicon slag, white carbon black and applications thereof. Background Art

[0002] The process of producing anhydrous hydrogen fluoride by the fluorosilicic acid method often produces a large amount of by-product - fluorine-containing silicon slag. Due to its relatively complex impurity composition, direct washing, drying and other methods cannot achieve efficient separation and utilization. If it cannot be effectively treated, it will seriously pollute the environment.

[0003] The existing technology often uses fluorine-containing silicon slag to produce white carbon black products to achieve efficient utilization of fluorine and silicon resources. White carbon black is hydrated silicon dioxide, which has the characteristics of high purity, small particle size and uniform dispersion, excellent optical properties and mechanical properties. The existing preparation methods of white carbon black are mainly divided into physical methods and chemical methods. The chemical method mainly includes precipitation method, gas phase method, gel method and microemulsion method, among which the gas phase method and precipitation method are commonly used methods for preparing white carbon black. The white carbon black prepared by the gas phase method has a large specific surface area, the product purity can reach 99%, and the particle size can reach 10-20nm, but the reaction process of this method is complicated, and the product price is expensive, and it is only used in a very small number of special industries. The traditional precipitation method refers to the process of producing white carbon black with sulfuric acid, hydrochloric acid, and water glass as basic raw materials. It has high output, simple process, and is easy to form a scale and is widely used, but this method has the problems of poor product dispersibility and insufficient specific surface area, and there is little research on the flow properties of white carbon black. Therefore, if the fluorine-containing silicon slag produced in the process of producing anhydrous hydrogen fluoride by the fluorosilicic acid method is utilized as a resource to produce white carbon black products with better quality, dispersion and fluidity, it will not only be of great significance to environmental protection, but also have better economic benefits. Summary of the invention

[0004] In order to solve the defects in the prior art, the present invention provides a method for producing white carbon black from fluorine-containing silicon slag, white carbon black and its application. The present invention is aimed at effectively treating the fluorine-containing silicon slag produced in the process of producing anhydrous hydrogen fluoride by the fluosilicic acid method. The fluorine and silicon yields of the process of preparing white carbon black from the fluorine-containing silicon slag by the production method of the present invention are high, and the obtained white carbon black product has excellent quality, good dispersibility and fluidity.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for producing white carbon black from fluorine-containing silicon slag, comprising the following steps:

[0007] S1, mixing sodium carbonate and sodium hydroxide and reacting with fluorine-containing silicon slag to obtain a fluorine-containing sodium silicate mixed solution, and then adding a surfactant to the mixed solution;

[0008] S2. CO2 gas is introduced into the fluorine-containing sodium silicate mixed solution to which a surfactant is added for reaction, and the reactant is separated into solid and liquid. After washing the obtained solid phase, n-butanol is added, mixed and dried.

[0009] Preferably, the chemical composition of the fluorine-containing silicon slag is calculated by mass percentage: total fluorine 7-7.5%, chloride ion 0.05-0.1%, sulfate 0.1%, phosphate 0.05-0.1%, water 60.75-62%, and silicon dioxide 30.25-32%.

[0010] Preferably, the mass ratio of the sodium carbonate, sodium hydroxide and fluorine-containing silicon slag in S1 is (13-27): (273-352): 1000.

[0011] Preferably, the reaction temperature in S1 is 100° C. and the reaction time is 3 min.

[0012] Preferably, the chemical composition of the fluorine-containing sodium silicate mixed solution in S1, measured in mass percentage, includes: 5-16% silicon dioxide, 7-21% sodium silicate solution, 1.8-5% sodium oxide, and 0.03-0.5% fluorine.

[0013] Preferably, the modulus of the fluorine-containing sodium silicate mixture is 2 to 3.2.

[0014] Preferably, the added amount of the surfactant is 2 to 3.5 g / L.

[0015] Preferably, the temperature of the fluorine-containing sodium silicate mixed solution in S2 is raised to 50-100° C. before reacting with CO 2 gas.

[0016] Preferably, during the S2 reaction, the flow rate of CO2 gas is 100-200 ml / min.

[0017] Preferably, CO2 gas is introduced into the S2 to react until the pH of the system drops to 8-10.

[0018] Preferably, in S2, the reactants are aged first and then solid-liquid separated.

[0019] Preferably, the aging time in S2 is 30 min.

[0020] Preferably, in the washing process S2, at least part of the washing steps are washed with an acidic solution.

[0021] Preferably, the amount of n-butanol added is 1.5-4.5% of the mass of the solid phase.

[0022] In a second aspect, the present invention provides a white carbon black product prepared by the above preparation method.

[0023] In a third aspect, the present invention also provides an application of the above-mentioned white carbon black product in the process of preparing water absorbents for rubber, coatings, inks, cosmetics, and food packaging.

[0024] The beneficial effects of the present invention are:

[0025] The production method of the present invention is to first react a mixture of fluorine-containing silicon slag with sodium carbonate and sodium hydroxide to obtain a fluorine-containing sodium silicate mixed solution, wherein the free fluorine in the fluorine-containing silicon slag reacts with sodium carbonate to generate sodium fluoride and carbon dioxide, and releases gas at the same time, which helps the mixing and diffusion of substances in the system, and the sodium hydroxide reacts with the crystallized fluorine and silicon dioxide in the fluorine-containing silicon slag to generate sodium fluoride and sodium silicate. In this process, the concentration of the system increases, which promotes the reaction rate and efficiency, thereby ensuring that the fluorine element is fully combined with the sodium ion, facilitating subsequent solid-liquid separation, and realizing efficient fluorine recovery. Subsequently, a surfactant is added to enhance the performance of the reaction medium, optimize the kinetic characteristics of the entire reaction system, and ensure more efficient material transmission and reaction rate. Then carbon dioxide is introduced into the system to promote the generation of silicon dioxide and sodium carbonate, thereby improving the yield of silicon dioxide, and in addition, it also helps to improve the dispersibility and fluidity of the final product. Finally, the impurities in the product are effectively removed through the washing process. As a good solvent, n-butanol can penetrate into the interior of the silica particles, replace the water therein, reduce the structural damage caused by the rapid evaporation of water during direct drying, improve the interaction between particles and reduce aggregation, enhance the fluidity of silica, and ensure that silica has excellent physical and chemical properties and meets the strict requirements of high-end application fields.

[0026] The white carbon black product prepared by the invention has rich surface structure, excellent dispersibility and fluidity, high product quality, and the rubber product prepared by using the white carbon black product has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The SEM images of the white carbon black prepared in Example 7 of the present invention and the commercially available white carbon black (a is the product obtained in Example 7, and b is the commercially available white carbon black product);

[0028] Figure 2 This is an infrared spectrum detection diagram of the white carbon black product prepared in Example 7 of the present invention;

[0029] Figure 3 This is the infrared spectrum detection diagram of the white carbon black product prepared by the gas phase method;

[0030] Figure 4 This is an infrared spectrum detection diagram of the white carbon black product prepared in Comparative Example 6;

[0031] Figure 5 This is the infrared spectrum detection diagram of the white carbon black product prepared in Comparative Example 7. DETAILED DESCRIPTION

[0032] In order to enable those skilled in the art to better understand the technical solution of the invention, the present invention is further described in detail below in conjunction with specific implementation methods.

[0033] In order to effectively treat the fluorine-containing silicon slag produced in the process of producing anhydrous hydrogen fluoride by the fluorosilicic acid method, the present invention uses the fluorine-containing silicon slag to produce white carbon black products. The process of the present invention has high fluorine and silicon yields, and the obtained white carbon black product has excellent quality, good dispersibility and fluidity. To achieve the above purpose, the present invention first proposes a method for producing white carbon black from fluorine-containing silicon slag, comprising the following steps:

[0034] S1, mixing sodium carbonate and sodium hydroxide and reacting with fluorine-containing silicon slag to obtain a fluorine-containing sodium silicate mixed solution, and then adding a surfactant to the mixed solution;

[0035] S2. CO2 gas is introduced into the fluorine-containing sodium silicate mixed solution to which a surfactant has been added for reaction, and the reactant is separated into solid and liquid. After washing the obtained solid phase, n-butanol is added, mixed and dried to obtain the product.

[0036] The present invention focuses on the efficient extraction and utilization of key chemical components from fluorine-containing silicon slag, aiming to improve the quality and yield of the product while reducing environmental impact. Specifically, this process involves multiple carefully designed steps to optimize the interaction between the components to achieve the best resource utilization efficiency and environmental benefits.

[0037] First, the free fluorine in the fluorine-containing silicon slag reacts with sodium carbonate to generate sodium fluoride and carbon dioxide, while releasing gas, which helps the mixing and diffusion of substances in the system. Sodium hydroxide reacts with crystalline fluorine and silicon dioxide in the fluorine-containing silicon slag to generate sodium fluoride and sodium silicate. In this process, the concentration of the system increases, providing better conditions for effective collisions between ions, promoting the reaction rate and efficiency, thereby ensuring that the fluorine element and sodium ions are fully combined to form solid sodium fluoride, which is convenient for subsequent solid-liquid separation and achieves efficient fluorine recovery. Subsequently, surfactants are added to enhance the performance of the reaction medium, while reducing energy consumption in subsequent processing, and optimizing the kinetic characteristics of the entire reaction system, ensuring more efficient material transfer and reaction rate.

[0038] Then, carbon dioxide is introduced into the system. Since the concentration of the system is relatively high at this time, carbon dioxide can contact sodium silicate more fully, promoting the formation of silicon dioxide and sodium carbonate, thereby increasing the yield of silicon dioxide. At this time, the sodium silicate solution tends to form a more uniform particle structure, which also helps to improve the dispersibility and fluidity of the final product.

[0039] Finally, through the washing process, impurities in the product are effectively removed, ensuring that silica has excellent physical and chemical properties and meets the strict requirements of high-end application fields. Silica usually contains a lot of water during the synthesis process. Direct drying may cause uneven evaporation of water inside the particles, resulting in unstable pore structure or particle agglomeration. As a good solvent, n-butanol can penetrate into the silica particles, replace the water therein, and reduce the structural damage caused by rapid evaporation of water during direct drying. After using n-butanol for solvent replacement, the drying rate of silica will be significantly accelerated. This is because the rapid evaporation of n-butanol takes away a lot of latent heat, accelerates the drying process, ensures that silica has excellent physical and chemical properties, and meets the strict requirements of high-end application fields. In addition, the design of the entire production process focuses on energy conservation and emission reduction, greatly reducing the generation of wastewater, embodying the principles of green chemistry, and making positive contributions to environmental protection.

[0040] The present invention is directed to fluorine-containing silicon slag produced in the process of producing anhydrous hydrogen fluoride by the fluosilicic acid method. The fluorine-containing silicon slag is alkaline, and its chemical composition is calculated by mass percentage: total fluorine 7-7.5% (including free fluorine 0.5-1%), chloride ion 0.05-0.1%, sulfate 0.1%, phosphate 0.05-0.1%, water 60.75-62%, silicon dioxide 30.25-32%. Under the chemical composition of the fluorine-containing silicon slag, the production process of the present invention can better react all silicon dioxide and improve the yield of fluorine and silicon.

[0041] In the reaction process described in S1 of the present invention, the mass ratio of sodium carbonate, sodium hydroxide and fluorine-containing silicon slag described in S1 is (13-27): (273-352): 1000. Further, the mass ratio of sodium carbonate, sodium hydroxide and fluorine-containing silicon slag is (13.25-26.5): (273.33-351.67): 1000.

[0042] In some embodiments of the present invention, the reaction temperature in the reaction process described in S1 is 100° C. and the reaction time is 3 min.

[0043] In the present invention, the chemical composition of the fluorine-containing sodium silicate mixed solution is measured by mass percentage, including: 5-16% silicon dioxide, 7-21% sodium silicate solution, 1.8-5% sodium oxide, and 0.03-0.5% fluorine. In some embodiments of the present invention, the mass content of silicon dioxide is any one of 5%, 7.5%, 10%, 15.98%, or a value between the two; the mass content of the sodium silicate solution is any one of 7.2%, 7.3%, 11%, 14.6%, 20.46%, or a value between the two; the mass content of sodium oxide is any one of 1.8%, 2.3%, 2.7%, 3.5%, 4.95%, or a value between the two; the mass content of fluorine is any one of 0.03%, 0.18%, 0.27%, 0.36%, 0.5%, or a value between the two. If the chemical composition in the fluorine-containing sodium silicate mixed solution exceeds the range value specified in the present invention, then too low a concentration will lead to a decrease in reaction efficiency, an increase in the amount of wastewater generated, a smaller particle size of the produced silicon dioxide and a decrease in yield; too high a concentration will lead to an increase in the viscosity of the reaction solution, an increase in the solid content, and poor fluidity, which is not conducive to stirring, mixing and mass transfer, and the product is more likely to agglomerate and difficult to disperse, affecting the processing operation and the uniformity of the final product, thereby affecting the reaction yield and product quality, and also causing an increase in the amount of wastewater.

[0044] The present invention limits the modulus of the fluorine-containing sodium silicate to 2 to 3.2 (the modulus refers to the ratio of SiO2 to Na2O in the silicate solution). A higher modulus means that the content of sodium silicate is relatively high, which is conducive to the generation of more silicon dioxide in the subsequent carbon dioxide reaction, thereby increasing the yield of silicon dioxide. In addition, a high modulus also helps to improve the dispersibility and fluidity of the final product, because a silicate solution with a high modulus tends to form a more uniform particle structure. In some embodiments of the present invention, the modulus of the fluorine-containing sodium silicate is any one of 2.17, 2.77, 2.85, and 3.2 or a value between the two. Too high a modulus sodium silicate is difficult to prepare, the reaction activity may be low, the carbonization reaction rate is slow, and a higher temperature or a longer reaction time is required to complete the conversion; too low a modulus leads to incomplete reaction, resulting in low fluorine and silicon yields, and the structure of the white carbon black generated by the reaction may be relatively loose, with a small specific surface area, weakened adsorption capacity and reinforcement effect, low product quality, and additional wastewater volume. Due to the high sodium ion content, residual sodium salt impurities may also increase, affecting the electrical insulation and other application properties of the product.

[0045] The surfactant of the present invention can significantly reduce the surface tension of the liquid and the solid-liquid interfacial tension, which helps to improve the solid-liquid contact state, promote the dispersion of solid particles, form a more uniform suspension, improve product performance indicators, and improve the mixing efficiency and material transfer rate of the reaction medium, and improve the fluorine yield. In the present invention, the amount of surfactant added is 2 to 3.5 g / L. In some embodiments of the present invention, the amount of the surfactant added is any one of 2g / L, 2.5g / L, 3g / L, 3.5g / L or a value between the two. In some embodiments of the present invention, the surfactant is PEG6000.

[0046] In S2 of the present invention, the temperature of the sodium silicate fluoride mixture is raised to 50-100°C before reacting with CO2 gas. In some embodiments of the present invention, the temperature of the sodium silicate fluoride mixture is raised to any one of 50°C, 80°C, 85°C, 90°C, 100°C or a value between the two. Temperature directly affects the formation and growth rate of white carbon black nuclei. When the reaction temperature is too low, the viscosity of the solution is high, which is not conducive to the movement of single particles and the relative movement between clusters composed of many particles. Small particles are easy to condense. When the reaction temperature is increased, the viscosity of the solution is reduced, and the Brownian motion of the particles is also intensified, which helps to produce loose white carbon black with higher oil absorption value and specific surface area; when the reaction temperature is too high, the viscosity of nano white carbon black is low, the Brownian motion of small particles and clusters is accelerated, the growth rate of the nucleus is also accelerated, and particles with larger particle sizes are easily produced. Clusters are easy to collide and aggregate to form large gels, which will reduce the oil absorption value, reduce the quality of white carbon black, and increase energy consumption.

[0047] In the present invention, it is also necessary to strictly control the gas flow rate when the CO2 gas is introduced. An appropriate gas velocity can ensure the uniform distribution of carbon dioxide in the fluorine-containing sodium silicate mixed solution, increase the contact opportunity of carbon dioxide and sodium silicate, and promote the process of carbon dioxide and sodium silicate reacting to generate silicon dioxide and sodium carbonate. Too fast or too slow gas velocity is not conducive to the full progress of the reaction. The present invention limits the flow rate of CO2 gas to 100-200ml / min. In some embodiments of the present invention, the flow rate of the CO2 gas is any one of 100ml / min, 150ml / min, 160ml / min, 200ml / min, or a value between the two. The gas flow rate specified in the present invention allows a relatively appropriate reaction time for generating silica, relatively slow crystal nucleation, and more complete agglomeration, which is conducive to the formation of uniform and stable silica particles; a flow rate that is too low may lead to incomplete reaction, affect the viscosity of the reaction system, and thus affect the fluorine and silicon yields; a flow rate that is too high may cause the generated primary particles to be quickly removed from the reaction zone before they have time to aggregate and grow, which is also not conducive to the formation of stable and high-quality white carbon black products and will also affect the fluorine and silicon yields.

[0048] The S2 of the present invention is introduced with CO2 gas to react until the pH of the system drops to 8 to 10. In some embodiments of the present invention, the pH of the reaction system of S2 is any one of 8, 8.5, 9, 9.5 or a value between the two.

[0049] In order to further improve the stability of the obtained white carbon black product, the reactants are aged before solid-liquid separation in S2. In some embodiments of the present invention, the aging time is 30 minutes.

[0050] In the washing process described in S2 of the present invention, at least part of the washing steps are washed with an acidic solution, which can be a sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid solution or a mixed solution. At least part of the washing steps are washed with an acidic solution so that the pH of the white carbon black product can reach the performance requirement of 5.0 to 8.0. Since the washing process reduces the residual impurities through pH adjustment, the white carbon black has better physical and chemical properties and meets the needs of high-end applications.

[0051] After washing S2 of the present invention, n-butanol is added to penetrate into the interior of the white carbon black particles, replace the water therein, and reduce the structural damage caused by the rapid evaporation of water during direct drying. The obtained white carbon black product has a rich surface structure, ensuring that the white carbon black has excellent physical and chemical properties, and the surfactant is used in combination with n-butanol to enhance the fluidity of the white carbon black by improving the interaction between particles and reducing aggregation. The amount of n-butanol added in the present invention is 1.5-4.5% of the mass of the solid phase. In some embodiments of the present invention, the amount of n-butanol added is any one of 1.5%, 3%, 4.5% of the mass of the solid phase, or a value between the two.

[0052] In a second aspect, the present invention also provides a white carbon black product prepared by the above preparation method.

[0053] In a third aspect, the present invention also provides an application of the above-mentioned white carbon black product in the process of preparing water absorbents for rubber, coatings, inks, cosmetics, and food packaging.

[0054] The above is a detailed description of the present invention, and the following are embodiments of the present invention.

[0055] Example 1

[0056] The fluorine-containing silicon slag involved in this embodiment comes from the fluorine-containing silicon slag produced in the process of producing anhydrous hydrogen fluoride by the fluorosilicic acid method of Guizhou Wengfu Lantian Fluorine Chemical Co., Ltd. The chemical composition of the fluorine-containing silicon slag is shown in Table 1 (total fluorine includes free fluorine).

[0057] Table 1 Unit wt%

[0058] <![CDATA[SiO2]]> Total Fluoride Free fluoride water Chloride ion Sulfate Phosphate 30.25 7.5 0.5 62 0.1 0.1 0.05%

[0059] This embodiment provides a method for producing white carbon black from fluorine-containing silicon slag, comprising the following steps:

[0060] (1) 13.25 kg of sodium carbonate and 351.67 kg of sodium hydroxide were mixed and reacted with 1 t of fluorine-containing silicon slag for 30 minutes at a temperature of 100° C. to obtain a reaction solution (the sodium silicate solution concentration in the reaction solution was 43.46%, the modulus was 2.15, the sodium oxide content was 13.97%, the silicon dioxide content was 30%, and the fluorine content was 0.2%). The silicon dioxide content in the reaction solution was diluted to 5% to obtain a fluorine-containing sodium silicate mixed solution (the sodium silicate solution concentration was 7.2%, the modulus was 2.17, the sodium oxide content was 2.3%, and the fluorine content was 0.03%), and then 3 g / L PEG6000 was added;

[0061] (2) The fluorinated sodium silicate mixed solution to which PEG6000 was added was heated to 80° C., and carbon dioxide gas was introduced at a gas flow rate of 100 ml / min. The reaction was terminated when the pH of the mixed solution dropped to 9.5. The mixed solution was stirred and aged for 30 min, and then filtered to obtain a filtrate and a solid phase. The filtrate was recycled separately, and the solid phase was washed three times, wherein the first and third washings were washed with 20 times of water, and the second washing was washed with a 5% dilute sulfuric acid solution until the pH was lower than 6.5. Finally, 3% of the mass of the solid phase after acid washing was added with n-butanol, mixed well, and dried to obtain the product.

[0062] Example 2

[0063] The same as Example 1, except that the gas flow rate in (2) is controlled at 150 ml / min, and the reaction is terminated when the pH of the mixed solution drops to 8.

[0064] Example 3

[0065] The same as Example 1, except that the gas flow rate in (2) is controlled at 160 ml / min, and the reaction is terminated when the pH of the mixed solution drops to 8.

[0066] Example 4

[0067] The same as Example 1, except that the gas flow rate in (2) is controlled at 200 ml / min, and the reaction is terminated when the pH of the mixed solution drops to 8.

[0068] Example 5

[0069] The fluorine-containing silicon slag involved in this embodiment comes from the fluorine-containing silicon slag produced in the process of producing anhydrous hydrogen fluoride by the fluorosilicic acid method of Guizhou Wengfu Lantian Fluorine Chemical Co., Ltd. The chemical composition of the fluorine-containing silicon slag is shown in Table 2.

[0070] Table 2 Unit wt%

[0071] <![CDATA[SiO2]]> Total Fluoride Free fluoride water Chloride ion Sulfate Phosphate 32 7 1 60.75 0.05 0.1 0.1

[0072] This embodiment provides a method for producing white carbon black from fluorine-containing silicon slag, comprising the following steps:

[0073] (1) 26.50 kg of sodium carbonate and 273.33 kg of sodium hydroxide were mixed and reacted with 1 t of fluorine-containing silicon slag for 30 minutes at a temperature of 100° C. to obtain a fluorine-containing sodium silicate mixed solution (sodium silicate solution concentration 20.46%, modulus 3.2, sodium oxide content 4.95%, silicon dioxide content 15.98%, fluorine content 0.5%), and then 3 g / L PEG6000 was added;

[0074] (2) The fluorinated sodium silicate mixed solution with PEG6000 added thereto is heated to 50° C., and carbon dioxide gas is introduced at a gas flow rate of 160 ml / min. The reaction is terminated when the pH value of the mixed solution drops to 9.5. The mixed solution is stirred and aged for 30 min, and then filtered to obtain a filtrate and a solid phase. The filtrate is recycled separately, and the solid phase is washed three times, wherein the first and third washings are washed with 20 times of water, and the second washing is washed with a 5% dilute sulfuric acid solution until the pH value is lower than 6.5. Finally, 3% of the mass of the solid phase after acid washing is added with n-butanol, mixed well, and dried to obtain the product.

[0075] Example 6

[0076] Same as Example 5, except that (2) the fluorine-containing sodium silicate mixed solution is heated to 100°C.

[0077] Example 7

[0078] Same as Example 5, except that (2) the fluorine-containing sodium silicate mixed solution is heated to 85°C.

[0079] Example 8

[0080] The same as Example 7, except that the reaction is terminated when the pH of the mixed solution in (2) drops to 8.5.

[0081] Example 9

[0082] The same as Example 5, except that the fluorine-containing sodium silicate mixed solution in (1) is diluted to a dilute solution with a silicon dioxide content of 5% (sodium silicate solution concentration 7.3%, modulus 2.77, sodium oxide content 1.8%, fluorine content 0.18%); (2) the fluorine-containing sodium silicate mixed solution is heated to 85° C., the gas flow rate is controlled at 160 ml / min, and the reaction is terminated when the pH of the mixed solution drops to 9.5.

[0083] Example 10

[0084] The same as Example 5, except that the fluorine-containing sodium silicate mixture in (1) is diluted to a dilute solution with a silicon dioxide content of 7.5% (sodium silicate solution concentration 11%, modulus 2.77, sodium oxide content 2.7%, fluorine content 0.27%).

[0085] Embodiment 11

[0086] The same as Example 5, except that the fluorine-containing sodium silicate mixture in (1) is diluted to a dilute solution with a silicon dioxide content of 10% (sodium silicate solution concentration of 14.6%, modulus 2.85, sodium oxide content of 3.5%, fluorine content of 0.36%).

[0087] Example 12

[0088] The same as Example 5, except that the amount of n-butanol added is 1.5% of the mass of the solid phase after pickling.

[0089] Embodiment 13

[0090] The same as Example 5, except that the amount of n-butanol added is 4.5% of the mass of the solid phase after pickling.

[0091] Embodiment 14

[0092] Same as Example 5, except that the added amount of PEG6000 is 2 g / L.

[0093] Embodiment 15

[0094] Same as Example 5, except that the added amount of PEG6000 is 2.5 g / L.

[0095] Example 16

[0096] Same as Example 5, except that the added amount of PEG6000 is 3.5 g / L.

[0097] Comparative Example 1

[0098] The process of Example 4 in patent CN112850722B has the following specific steps:

[0099] A method for preparing white carbon black and cryolite in steps using fluorine-containing silicon slag, the specific implementation steps are as follows:

[0100] (1) 50 g of fluorine-containing silicon slag was dissolved in 2000 mL of 60 g / L sodium hydroxide solution for 120 min, the temperature was controlled at 70° C., and insoluble impurities were removed by filtration to obtain a fluorine-containing sodium silicate solution A (the concentration of the sodium silicate solution was less than 5%, and the modulus was less than 0.5);

[0101] (2) CO2 was introduced into solution A at a rate of 12 mL / min until the pH of the solution at the end of the reaction was 10.0, and a silicon dioxide wet cake and a fluorine-containing sodium carbonate solution B were obtained after liquid-solid separation.

[0102] (3) The silicon dioxide wet cake is washed with distilled water until it becomes neutral and dried to obtain the white carbon black product.

[0103] Comparative Example 2

[0104] Same as Example 7, except that: the raw material composition of the fluorine-containing silicon slag is: 45.5% silicon dioxide, 12.5% ​​fluorine (including 2.3% free fluorine), 41.55% water, and 0.45% other. The modulus of the obtained fluorine-containing sodium silicate solution is 3.23, and the concentration of the sodium silicate solution is 20.46%.

[0105] Comparative Example 3

[0106] Same as Example 7, except that: (1) 45 kg of sodium carbonate and 450 kg of sodium hydroxide.

[0107] Comparative Example 4

[0108] The same as Example 7, except that the modulus of the fluorine-containing sodium silicate solution mixture obtained by adjusting (1) is 1, the concentration of the sodium silicate solution is 22.03%, the sodium oxide content is 10.98%, the silicon dioxide content is 11.05%, and the fluorine content is 0.67%.

[0109] Comparative Example 5

[0110] Same as Example 7, except that the gas velocity of the introduced carbon dioxide in (2) is controlled to be 10 ml / min.

[0111] Comparative Example 6

[0112] Same as Example 7, except that the gas velocity of the introduced carbon dioxide in (2) is controlled to be 300 ml / min.

[0113] Comparative Example 7

[0114] Same as Example 7, except that n-butanol is not added.

[0115] Comparative Example 8

[0116] Same as Example 7, except that PEG6000 is not added.

[0117] Effect Example 1 Fluorine Yield Detection

[0118] The fluorine yield and silicon yield in the production process of the embodiment and the comparative example were tested, and the data are shown in Table 3.

[0119] Table 3

[0120]

[0121]

[0122] It can be seen from Table 3 that the fluorine and silicon yields of the production method described in the embodiment of the present invention can reach more than 98%. In the production process of Comparative Example 1, the sodium silicate concentration is lower than 5%, and the modulus is lower than 0.5. Due to the excessive dilution of the reaction system, the reaction is insufficient, the silicon slag is not completely dissolved, and secondary solid waste is generated. The fluorine yield is 96%, and the silicon yield is lower than 96%. In Comparative Example 2, since the fluorine-containing silicon slag raw material is different from the present invention, that is, it exceeds the limited range of the chemical composition of the fluorine-containing silicon slag raw material defined in the present invention, the silicon dioxide cannot be fully reacted, and part of the fluorine-containing silicon slag does not react, which will lead to a decrease in the fluorine and silicon yields, especially a significant decrease in the silicon yield. In the production process of Comparative Example 3, due to the excessive viscosity of the system caused by the excessive alkali, the reaction generation is uneven, resulting in a decrease in the fluorine and silicon yields. Due to the reduced modulus, Comparative Example 4 cannot react completely with the corresponding mass of alkali, resulting in incomplete reaction of silicon dioxide, and the fluorine and silicon yields will be reduced, especially the silicon yield is greatly reduced. In Comparative Example 5, since the carbon dioxide gas velocity is lower than the limited range of the present invention, the reaction time is long, the water evaporates continuously, the viscosity of the system of the subsequent reaction increases, and part of the sodium silicate solution is unreacted, resulting in a decrease in the yield of fluorine silicon. In Comparative Example 6, since the carbon dioxide gas velocity is higher than the limited range of the present invention, the generated particle size is finer, the filtration process is perforated, and the yield decreases. In Comparative Example 7, n-butanol is not added, because it is added in the drying stage, so there is no substantial change in the yield. In Comparative Example 8, PEG6000 is not added, because the surfactant can significantly reduce the liquid surface tension and the solid-liquid interfacial tension, which helps to improve the solid-liquid contact state, promote the dispersion of solid particles, and form a more uniform suspension, thereby improving the mixing efficiency and material transfer rate of the reaction medium, and thus the silicon yield is reduced.

[0123] Effect Example 2: Physical and Chemical Properties of White Carbon Black

[0124] The physical and chemical properties of the white carbon black produced in the examples and comparative examples were tested, and the data are shown in Table 4.

[0125] Table 4

[0126]

[0127]

[0128] It can be seen from Table 4 that the white carbon black product prepared in the embodiment of the present invention has excellent quality and meets the national standard requirements. It can be seen from Comparative Example 2 that exceeding the limit of the content of the chemical composition of the fluorine-containing silicon slag of the present invention will result in the product elongation at break, oil absorption value lower than the national standard and oil absorption value lower than the national standard requirements, and the product quality is unqualified. It can be seen from the data of Comparative Example 3 that if the amount of sodium carbonate and sodium hydroxide exceeds the range specified by the present invention, the tensile strength and elongation at break will not meet the national standard requirements, and it is an unqualified product. It can be seen from Comparative Example 4 that if the modulus of the fluorine-containing sodium silicate solution and the concentration of the fluorine-containing sodium silicate are less than the range specified by the present invention, the white carbon black structure generated by the reaction will be relatively loose, the specific surface area will be small, the oil absorption value will decrease, the adsorption capacity and reinforcement effect will be weakened, and it will be an unqualified product. It can be seen from Comparative Example 5 that too low a carbon dioxide gas velocity will result in a smaller surface area, reduce the crosslinking density and rigidity of the white carbon black, increase the rubber, limit the slip and extension of the molecular chain, thereby making the rubber harder and more brittle, and reducing the tensile strength and elongation at break. It can be seen from Comparative Example 6 that the oil absorption value of the product obtained when the carbon dioxide gas velocity is too high does not meet the standard. Low oil absorption value will affect the uniformity and performance of rubber products, reduce the crosslinking density, weaken the physical properties of rubber, and lead to a decrease in indicators such as tensile strength. It can be seen from Comparative Example 7 that no n-butanol was added, and the water inside the silica particles evaporated unevenly during the drying process, resulting in an unstable pore structure or particle agglomeration, resulting in its performance indicators not meeting the requirements. Comparative Example 8 did not add PEG6000, and the particles agglomerated during the silica generation process, resulting in some product indicators being unqualified.

[0129] Effect Example 3: Dispersibility Test of White Carbon Black Products

[0130] The white carbon black product prepared in Example 7 was characterized by SEM. Figure 1 , wherein a is the SEM image of the product obtained in Example 7, and b is the commercially available white carbon black product prepared by the sulfuric acid method (with the same physical and chemical properties as the product obtained in Example 7). It can be seen from the figure that under the same magnification conditions, the white carbon black prepared by the present invention has a finer particle size and is more evenly dispersed, indicating that the product of the present invention has higher dispersibility.

[0131] Effect Example 4 Fluidity Test of White Carbon Black Products

[0132] Test method: Place a 20cm PVDF plate at an angle of 30 degrees to the horizontal plane, place 100g of white carbon black product on the top, and calculate the time for it to flow downward from the top. The results are shown in Table 5.

[0133] Table 5

[0134]

[0135] From the results in Table 5, it can be seen that compared with the white carbon black in Comparative Examples 7 and 8, which only added PEG6000 or n-butanol, the fluidity of the products obtained in Examples 5, 7, and 12 is significantly better. Compared with the commercially available white carbon black prepared by the sulfuric acid method, the white carbon black product prepared by the present invention also has better fluidity. This shows that adding PEG and n-butanol in appropriate amounts can enhance the fluidity of white carbon black by improving the interaction between particles and reducing aggregation. The particle morphology of the white carbon black prepared by the sulfuric acid method may not be uniform enough, and the particle size is large, resulting in a strong interaction force between particles, which is easy to form agglomerations, thereby reducing the fluidity of the material.

[0136] Effect Example 5: Characterization of the structure of white carbon black products

[0137] The white carbon black product obtained in Example 7 was compared with the white carbon black prepared by the conventional gas phase method of the same specification (the physical and chemical properties of the product obtained in Example 7 are the same as those of the product obtained in Example 7) and Comparative Example 6 and Comparative Example 7. The product quality is shown in Table 6 and the infrared spectrum is shown in Figure 2 to Figure 5 (in, Figure 2 This is the infrared spectrum detection diagram of the white carbon black product prepared in Example 7 of the present invention, Figure 3 This is the infrared spectrum detection diagram of the white carbon black product prepared by the gas phase method. Figure 4 This is the infrared spectrum detection diagram of the white carbon black product prepared in Comparative Example 6, Figure 5 This is the infrared spectrum detection diagram of the white carbon black product prepared in Comparative Example 7).

[0138] Among them, the process of preparing white carbon black by gas phase method is: using organic silane halide as raw material, hydrolyzing it at high temperature (generally up to 1200-1600℃) in hydrogen and oxygen flames to generate extremely fine smoke-like SiO2 particles; the smoke-like SiO2 is integrated into larger particles in the aggregator, and then collected into the deacidification furnace through a cyclone separator for deacidification treatment to obtain the obtained product.

[0139] Table 6

[0140]

[0141] It can be seen from Table 6 that the white carbon black product prepared by the present invention has higher tensile stress, tensile strength and elongation at break than the product of the same specification prepared by the gas phase method, indicating that the product prepared by the method of the present invention has better performance.

[0142] Figure 2 and Figure 3Comparison of the two figures shows that the absorbance of the product obtained in Example 7 is higher than that of fumed silica, and the types and number of surface hydroxyl structures displayed are significantly higher than those of fumed silica, indicating that the silica prepared by the present invention has a rich surface structure. The hydroxyl groups on the surface of the silica of the present invention can be connected to the rubber molecular chains through hydrogen bonding or chemical reactions to form physical or chemical crosslinking points, thereby enhancing the network structure of the rubber, especially the isolated hydroxyl groups and ortho-hydroxyl groups, which have high activity and can effectively react with the groups in the rubber, thereby significantly improving the tensile strength and modulus of the rubber. This reinforcement mechanism is based on the formation of a three-dimensional network structure, which improves the mechanical properties of the rubber. Figure 4 and Figure 5 It can be seen that when the gas velocity exceeds the specified range, the infrared spectrum shows that the surface structure type changes, which is specifically manifested by the peak 1630cm obtained by software analysis. -1 、966cm -1 The two structural peaks disappeared and the absorbance weakened. When n-butanol was not added in the process, the product obtained had a peak of 1630 cm -1 The peak disappears and the absorbance weakens, indicating that white carbon black products with rich surface structure and excellent performance can only be prepared under appropriate conditions and the presence of n-butanol.

[0143] Effect Example 6 Wastewater Quantity Detection

[0144] The amount of wastewater generated during the production process of the embodiments and comparative examples was statistically analyzed, and the data are shown in Table 7.

[0145] Table 7

[0146]

[0147]

[0148] It can be seen from Table 7 that the amount of wastewater generated during the production process of the embodiment of the present invention is between 16 and 18 tons, while according to the data of Comparative Example 1, 127.3 tons of wastewater are generated in the reaction step for every ton of product produced, and at least 100 tons of water are required to wash 1 ton of alkaline product to neutrality during the washing process. Comprehensive calculation shows that at least 227.3 tons of fluorine-containing wastewater are generated, which is much higher than the industry average of 80 tons of wastewater. Comparative Examples 2 to 6 also increase the amount of wastewater generated because the limited parameters exceed the limited range of the present invention.

[0149] Effect Example 7 Rubber Performance Applicability Test

[0150] The white carbon black product prepared in Example 7 was made into rubber by conventional methods in the art. The test indicators of the obtained rubber are shown in Table 8.

[0151] Table 8

[0152]

[0153]

[0154]

[0155]

[0156] It can be seen that the white carbon black prepared by the present invention is used to prepare rubber, and the obtained rubber has excellent quality.

[0157] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for producing white carbon black from fluorine-containing silicon slag, characterized in that: The following steps are involved: S1, mixing sodium carbonate and sodium hydroxide and reacting with fluorine-containing silicon slag to obtain a fluorine-containing sodium silicate mixed solution, and then adding a surfactant to the mixed solution; S2. CO2 gas is introduced into the fluorine-containing sodium silicate mixed solution to which a surfactant is added for reaction, and the reactant is separated into solid and liquid. After washing the obtained solid phase, n-butanol is added, mixed and dried.

2. The method according to claim 1, characterized in that The chemical composition of the fluorine-containing silicon slag is calculated by mass percentage: total fluorine 7-7.5%, chloride ion 0.05-0.1%, sulfate 0.1%, phosphate 0.05-0.1%, water 60.75-62%, and silicon dioxide 30.25-32%.

3. The method according to claim 1 or 2, characterized in that: The mass ratio of sodium carbonate, sodium hydroxide and fluorine-containing silicon slag in S1 is (13-27): (273-352): 1000.

4. The method according to claim 1 or 2, characterized in that: The chemical composition of the sodium fluoride silicate mixed solution in S1, measured in mass percentage, includes: 5-16% silicon dioxide, 7-21% sodium silicate solution, 1.8-5% sodium oxide, and 0.03-0.5% fluorine.

5. The method according to claim 1, characterized in that The added amount of the surfactant is 2-3.5 g / L.

6. The method according to claim 1, characterized in that During the reaction process described in S2, the flow rate of CO2 gas is 100-200 ml / min.

7. The method according to claim 1, characterized in that In the washing process S2, at least part of the washing steps are performed using an acidic solution.

8. The method according to claim 1 or 7, characterized in that: S2: The amount of n-butanol added is 1.5-4.5% of the mass of the solid phase.

9. A white carbon black product produced by the production method according to any one of claims 1 to 8.

10. Use of the white carbon black product according to claim 9 in the process of preparing water absorbents for rubber, coatings, inks, cosmetics, and food packaging.

Citation Information

Patent Citations

  • A method for stepwise preparation of silica and cryolite from fluorinated silica slag

    CN112850722B

  • Method for separating sodium fluoride crystals from silicon dioxide

    CN101717097A

  • Method for preparing white carbon black from silicon slags containing fluorine

    CN103663474A

  • Method for preparing nano white carbon black through residues generated after aluminum oxide acid leaching extraction of coal ash and slag

    CN105197937A

  • Method for preparing white carbon black and cryolite step by step from fluorine-containing silicon slag

    CN112850722A