Treatment process for smelting high-chlorine material by using noble metal

By using evaporation and physical separation methods to process high-chlorine materials in non-ferrous smelting, the problem of difficult precious metal recovery has been solved, achieving efficient recovery and harmless treatment of resources, simplifying the process flow and reducing processing costs.

CN118878129AActive Publication Date: 2024-11-01HENAN ZHONGYUAN GOLD SMELTERY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410980129.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-01
Estimated Expiration
2044-07-22

Smart Images

  • Figure CN118878129A_ABST
    Figure CN118878129A_ABST
Patent Text Reader

Abstract

The invention discloses a treatment process for smelting a high-chlorine material by using noble metal. The process is mainly divided into four process stages: (1) concentration stage; (2) an evaporation separation stage; (3) a precious metal recovery stage; and (4) a circulation stage. In the precious metal recovery process, a physical separation method is introduced to separate chlorine and precious metal ions in materials, the problems that under the conditions of high-concentration chloride ions and acidity, the chemical method agent dosage is large, and waste water is difficult to treat are solved, the waste water is effectively treated, harmful chlorine is recovered into recyclable hydrochloric acid, and the waste water is recycled. Moreover, valuable elements which are very low in concentration and even difficult to detect can be recycled, high-grade and easy-to-recycle precious slag is obtained, precious metal is basically not lost, compared with adsorbents such as activated carbon and resin, the technological indexes are more stable, and precious metal recycling is easier and more convenient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nonferrous metal and precious metal smelting, and in particular relates to a treatment process for high-chloride materials in precious metal smelting. Background Art

[0002] The chlorine-containing materials include both solid and liquid types, and are mainly targeted at various waste liquids and waste slags whose main components are soluble chloride salts. Similar intermediate materials may also be applicable. In the field of non-ferrous smelting, chlorine, sodium chloride, perchloric acid, sodium hypochlorite, sodium chlorate and other chlorine-containing agents are widely used in industrial production, during which a large amount of chlorine-containing materials are inevitably generated and need to be treated. Since the non-ferrous industry usually involves a large number of restricted emission elements, such materials often have a complex composition. Chloride ions, as a very strong chelating agent, will greatly increase the difficulty of wastewater treatment even if their concentration is only about 1g / L, and it is difficult to meet the external discharge indicators.

[0003] At present, the amount of such waste liquid and waste residue is generally small, but due to the common existence of multiple elements in the non-ferrous industry, with the development of science and technology in recent years, the refining technology has also made great progress. When achieving comprehensive recovery of multiple elements, the process is often complicated, resulting in a wide variety of wastewater and waste residues with large differences in composition. Commonly used chlorine-containing wastewater treatment methods such as ion exchange, ultrafiltration, reverse osmosis, electrolysis, electrodialysis and other methods are difficult to treat various types of wastewater at the same time, which severely limits their application. Liquids are usually treated as ordinary industrial wastewater after recovering trace amounts of valuable elements using methods such as adsorption and sulfidation, and then reused or discharged. For example, the chloride ion concentration in the wastewater produced by the chlorination gold leaching process can reach 100g / L, and it often contains high concentrations of salt and trace amounts of precious metal elements such as Au, Ag, Pt, Pd, etc. Since it cannot be directly reused, in order to recover the precious metals, activated carbon adsorption and other methods are often used for simple treatment. However, due to factors such as high ion concentration, active site adsorption saturation, and difficulty in analysis and detection, the treatment indicators are often difficult to control. The recovery of precious metals adsorbed on activated carbon also has high technical difficulties, and the precious metal resources remaining in the liquid after adsorption are also wasted. Solids generally also contain valuable elements and are difficult to treat as ordinary solid wastes. Only more targeted special methods can be designed separately. However, similar to liquids, they also have the characteristics of "small amount", "many types", and "complex composition". They are usually returned to the system for treatment, and long-term circulation is difficult to avoid the accumulation of harmful elements.

[0004] Traditional water treatment processes generally use lime or quicklime as an adjusting agent. During the treatment process, most valuable elements generally sink into the slag together, causing a waste of resources. Since chloride ions are difficult to enter the slag, the treated water has high heavy metal content, high hardness that is difficult to reduce, and high salinity. Reuse will cause a series of problems, such as equipment and facility corrosion, valuable metal dissolution, equipment and pipeline scaling, etc. This type of impact is difficult to reflect in the short term and is often ignored, which invisibly increases production costs. Traditional evaporation processes are rarely used due to their high costs, and research is mainly aimed at relatively pure hydrochloric acid wastewater, mainly by adding magnesium chloride to destroy the azeotropic composition of hydrochloric acid to recover high-concentration hydrochloric acid. The particularity of wastewater in the non-ferrous industry makes it difficult to directly apply. Summary of the invention

[0005] The purpose of the present invention is to provide a processing technology for high-chlorine materials in precious metal smelting, which can coordinately process a variety of chlorine-containing materials, use an evaporation process, and recycle chlorine as hydrochloric acid. The low-content precious metals contained in the materials are finally recovered in solid form after enrichment, which has an excellent effect on recovering low-concentration high-value precious metal resources.

[0006] The chlorine-containing material is a liquid or solid in which chlorine mainly exists in the form of -1 valence or in the form of -1 valence after mixed treatment.

[0007] To achieve the above purpose, Figure 1 As shown, the present invention adopts the following technical solutions:

[0008] This process is mainly divided into four process stages: (1) concentration stage; (2) evaporation separation stage; (3) precious metal recovery stage; (4) circulation stage.

[0009] (1) Concentration stage

[0010] The purpose of this stage is to reduce the amount of low-concentration liquid entering the evaporation separation stage without affecting the recovery of precious metals, thereby reducing the amount of liquid that needs to be evaporated, reducing processing costs and increasing the concentration of hydrochloric acid obtained, without affecting the subsequent recovery of precious metals. When the total soluble chlorine in the liquid after the chlorine-containing materials to be treated is above 100g / L (chlorine ions can be well volatilized after exceeding this concentration), this stage can be skipped. When the total soluble chlorine in the liquid after the chlorine-containing materials to be treated is less than 100g / L or even when the total soluble chlorine in the liquid after the chlorine-containing materials to be treated is above 100g / L, the following operations are performed for the chlorine-containing liquid in which the chloride ion concentration is lower than 100g / L:

[0011] a. Sort the chlorine-containing liquids having a chloride ion concentration of less than 100 g / L by acidity (the acidity in this application refers to the concentration of hydrochloric acid), with the lower one or more as chlorine-containing liquid A, and the remaining chlorine-containing materials as chlorine-containing material B;

[0012] b. Separating and enriching the chloride ions in the chlorine-containing liquid A to obtain an enriched liquid C and a dechlorinated liquid D;

[0013] Since precious metals generally exist in the form of chlorine complex ions in chlorine-containing liquids, they will enter the enriched liquid C together with chlorine during the enrichment process. The dechlorinated liquid D can be treated as ordinary wastewater, and the concentration end point can be reasonably selected according to different requirements for the dechlorinated liquid, without affecting the subsequent process.

[0014] (2) Evaporation separation stage

[0015] This stage is the key stage of the present invention. First, the chlorine-containing substance B, the enriched liquid C and the circulating liquid H are sent to the evaporation crystallization device for mixing, and then the reagent E is added according to the amount and quality of the precious metals to be recovered in the mixed liquid. Since the concentration of precious metals in the wastewater is often very low and the detection deviation is often large, the general addition amount does not exceed the theoretical required amount to prevent the waste of reagents and affect the quality of the recovered material. The recommended addition amount is 0.1 to 0.9 times the theoretical required amount, and is adjusted according to the change trend of the concentration of precious metals to be recovered in the subsequent evaporation residual liquid.

[0016] If the acid / chlorine molar ratio after mixing is less than 1, then add reagent F, otherwise it is not necessary to add. The higher the acid / chlorine molar ratio, the more conducive it is to reduce the concentration of chloride ions in the evaporation residue, but too high a ratio will cause the hydrochloric acid to volatilize in the form of HCl gas instead of in the form of azeotrope. The acid / chlorine molar ratio is generally controlled at 1 to 3, and more preferably, the acid / chlorine molar ratio is 1 to 2.

[0017] The mixed liquid is heated and evaporated, and most of the chloride ions are volatilized as hydrochloric acid vapor, and hydrochloric acid is obtained after condensation. The remaining non-volatile matter is further concentrated and enriched in this process.

[0018] (3) Precious metal recovery stage

[0019] If the treated material contains selenium, part of it may enter the gas phase with the hydrochloric acid vapor, and finally be recovered together with the condensed hydrochloric acid. The hydrochloric acid is separated into liquid and solid to obtain crude selenium solid; after the chlorine-containing material is concentrated and enriched, the concentration of each element is increased. As the concentration of chloride ions is reduced, the precious metals dissolved by the complexation of chloride ions are released. Even at very low concentrations, they can react with the reagent E in the solution under the thermal environment of evaporation, and precipitate from the liquid with soluble salts after exceeding the solubility, thereby obtaining a solid-containing residual liquid. The obtained residual liquid is separated by sedimentation to obtain a supernatant and a precious metal slurry. The precious metal slurry is centrifuged, and the filtrate is merged into the supernatant. The solid layer containing salt crystals is added with the dechlorination liquid D, stirred and dissolved, and then filtered to obtain precious slag and concentrated salt solution;

[0020] (4) Cycle stage

[0021] The circulation stage is the treatment and recycling of the supernatant and concentrated brine obtained from the precious slag treatment stage.

[0022] Concentrated brine circulation: Concentrated brine generally does not contain harmful elements and can be directly processed or circulated as a solvent to dissolve salt crystals. When it reaches a certain concentration, it is concentrated, cooled and crystallized. After the salt crystals are separated, the mother liquor is continuously circulated as a solvent. If the chloride ion concentration is high, it can also be treated as chlorine-containing waste liquid, or when the chloride ion concentration in the mother liquor reaches 100g / L or above, it can be incorporated into the supernatant for treatment.

[0023] Supernatant liquor circulation: When the content of precious metal elements in wastewater is low, a single treatment may not reach its precipitation concentration and remain in the residual liquid. Therefore, multiple cycles of enrichment are often required. Even if precipitation occurs, the residual liquid usually still contains a certain concentration of chlorine. Therefore, the supernatant obtained in the precious slag treatment stage still contains unprecipitated precious metals and other elements with recovery value. Directly opening the circuit will not only cause waste of resources but also reduce the chlorine recovery rate. Recycling can not only recover useful elements to the greatest extent, but also provide a basic driving force for the subsequent volatilization and precipitation of chloride ions. Due to the buffering effect of ions in the circulating liquid, the range of related reagent addition can be relaxed to a certain extent to reduce the difficulty of operation. During the circulation process, some valuable elements that are difficult to recover in the previous stages, or harmful elements that affect the volatilization of chloride ions may accumulate. In this case, the supernatant needs to be purified to prevent the system from being affected during the circulation process. According to the amount and type of impurities brought in by the chlorine-containing material being processed, a part or all of the circulating liquid H obtained by adding reagent G for purification in each circulation is separated to maintain the indicators of the evaporation separation stage within a reasonable range. If the amount brought in is small and the impact on the system is small, it can also be purified after a certain number of cycles. The minimum amount of reagent G added is the theoretical reaction amount required for the difference between the impurities in the supernatant and the circulating liquid added in stage (2), but the maximum amount does not exceed the theoretical reaction amount required for the impurities in the supernatant. It is recommended that the actual amount added does not exceed 0.8 times the maximum amount to prevent excessive purification agent from returning to the system, resulting in a decrease in the grade of precious slag or even difficulty in separation. This process may produce purified slag containing valuable elements, which can be recycled as concentrate.

[0024] Furthermore, in step (1), the precious metal in the chlorine-containing material is one or more of Au, Ag, Se, Cu, Te, Pt, Pd, and Rh.

[0025] Furthermore, in step (1), separation and enrichment of chloride ions in the chlorine-containing liquid A refers to separation and enrichment of chloride ions in the chlorine-containing liquid A by one or more of conventional evaporation concentration, ion exchange and membrane separation methods.

[0026] Furthermore, in step (2), the evaporation crystallization device includes but is not limited to an OSLO type crystallizer, a DTB type crystallizer, a common evaporator, a reactor and related improved types, or a combination of several of them.

[0027] Furthermore, in step (2), the reagent E includes but is not limited to one or more reducing agents or salts such as sulfurous acid, sodium chloride, sodium thiosulfate, sodium sulfite, metal elements, hydrazine hydrate, etc., and its main function is to react with the precious metal ions to be recovered to generate solids and precipitate from the solution.

[0028] Furthermore, in step (2), the agent F may include but is not limited to sulfuric acid, phosphoric acid, hydrochloric acid, hydrobromic acid, nitric acid, sulfurous acid, etc., which may provide H + of acids.

[0029] Furthermore, in step (4), the agent G includes but is not limited to one or a mixture of several of calcium carbonate, calcium oxide, sodium hydroxide, magnesium oxide, and sodium sulfide.

[0030] The acid / chlorine molar ratio in this application refers to the molar ratio of hydrochloric acid to chloride ions.

[0031] The innovation of this process is that in the process of precious metal recovery, a physical separation method is introduced to separate the chlorine and precious metal ions in the material, which overcomes the problem of large amount of chemical reagents used under high concentration of chloride ions and acidity conditions, and difficult wastewater treatment. This process not only effectively treats the wastewater and recovers harmful chlorine as reusable hydrochloric acid, but also recovers valuable elements with very low concentration or even difficult to detect, and obtains high-grade and easy-to-recover precious slag. There is basically no loss of precious metals. Compared with the use of adsorbents, such as activated carbon, resin and other process indicators are more stable, and precious metal recovery is simpler.

[0032] The beneficial effects of the present invention are as follows: the process comprehensively treats a variety of chlorine-containing materials at the same time, the process flow is simple and easy to implement, the recovery rate is high, and the disadvantage of poor selectivity of such materials is overcome. Not only liquids that were difficult to treat in the past, but even solid materials, especially difficult-to-treat materials containing controlled components, can be harmlessly treated through this process, and no new waste liquid is generated, which is economical and environmentally friendly. The present invention has good adaptability and can treat low-concentration precious metal chlorine-containing materials. While recovering hydrochloric acid, it can also enrich and recover the precious metals therein; it is particularly suitable for the separation and recovery of insoluble chlorine-containing compounds such as silver chloride, and good results can be obtained even at very low concentrations. In addition, the present invention can also be used alone as a high-concentration chlorine-containing material to recover chlorine BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0035] Embodiment 1:

[0036] There are two liquids, 1600mL chlorine-containing liquid 1# and 3200mL chlorine-containing liquid 2#. Both liquids also contain sodium sulfate, sulfuric acid and other ingredients. 400g NaCl mass fraction of about 90% solid chlorine-containing material 3# needs to be processed. Among them, chlorine-containing liquid 1# contains a high concentration of Ag, which is to be recovered. The material is processed in 4 times. The process is as follows:

[0037] (1) Concentration stage

[0038] The calculation shows that the chloride ion concentration of the three chlorine-containing materials after direct mixing is about 159g / L, which is greater than 100g / L, so it is not necessary to concentrate. However, since there is still liquid with a chloride ion concentration lower than 100g / L, and we want to obtain hydrochloric acid with a higher concentration, we concentrated it. The chloride ion of chlorine-containing liquid 1# is lower than 100g / L, and the acidity is the lowest. 400mL of chlorine-containing liquid 1# is evaporated and concentrated to about half of its volume. The evaporated gas is condensed and recovered to obtain a dechlorinated liquid with a chloride ion of only about 0.2g / L, as well as an unevaporated enriched liquid. The relevant results are shown in the table below.

[0039]

[0040] Note: The unit in Ag liquid is g / m 3 , and the rest of the units are g / L.

[0041] (2) Evaporation separation stage

[0042] Add the enriched liquid, 800mL of chlorine-containing liquid 2#, 100g of chlorine-containing material 3#, and the returned circulating liquid into a common evaporator and mix. Since the acid (hydrochloric acid) / chlorine molar ratio is about 1.04, which is greater than 1, no acid is added. Ag can form AgCl precipitation with chloride ions, and no reagent is needed. Se mainly exists in the form of selenite. To recover Se, a reducing agent needs to be added. Sodium sulfite is added here, and the theoretical addition amount is about 0.5g. Since the concentration is too low, in order to prevent the detection error and other effects, excessive addition of reagents is caused, and SO2 is generated to affect the quality of hydrochloric acid. Here, it is added at 0.6 times, and only 0.3g is added. In the subsequent circulation process, if the concentration has an increasing trend, the addition amount is gradually increased, and then heated and distilled, and the residual liquid volume is controlled at about 400mL. The steam is condensed to obtain slightly red hydrochloric acid, and red amorphous selenium and clarified hydrochloric acid are obtained after filtration.

[0043] (3) Precious metal recovery stage

[0044] The residual liquid obtained in step (2) is precipitated, and the supernatant is separated to obtain a precious metal slurry. There is an obvious boundary layer at the bottom of the precious metal slurry. Further centrifugal separation is performed, and the liquid is filtered out to obtain a crystalline slag. The slag is separated at a ratio of about 4:1 from top to bottom (slightly above the stratification point). The upper part is an anhydrous sodium sulfate layer. The bottom precious metal layer is taken and a dechlorination liquid at about 30° C. is used to basically dissolve the crystals, and then filtered to obtain an off-white precious slag with a silver chloride content of about 2wt%, and a sodium sulfate solution.

[0045] (4) Cycle stage

[0046] About 600 mL of the sodium sulfate solution obtained in step (3) is cooled to about 10° C. for crystallization, and the mother liquor after the sodium sulfate crystallization is filtered out as a solvent for subsequent precious metal layer treatment. The supernatant in step (3) and the centrifuged separation liquid are mixed, and sodium sulfide with a mass fraction of about 10% is added dropwise to remove Cu. The theoretical amount added is about 2 mL. Since the concentration is too low, in order to prevent the influence of detection errors, etc., excessive addition of the agent will produce harmful gas H2S. Here, 1.5 mL (about 0.75 times) is added. In the subsequent circulation process, if the concentration tends to increase, the amount added is gradually increased, and black copper sulfide slag is obtained by filtration. The filtrate is returned to the evaporation separation stage as a circulating liquid.

[0047] After all chlorine-containing materials were treated by repeating steps (1) to (4), a total of about 4400 mL of hydrochloric acid, about 0.6 g of red amorphous selenium, 0.9 g of black copper sulfide slag, 1.9 g of noble slag, and 380 mL of circulating liquid were obtained. The relevant results are shown in the table below.

[0048]

[0049] Note: The unit in Ag liquid is g / m 3 , and the rest of the units are g / L.

[0050] Embodiment 2:

[0051] There are two liquids that need to be processed: 100L chlorine-containing liquid 4# and 200mL mixed chlorine-containing liquid 5# of sulfuric acid and hydrochloric acid. Among them, chlorine-containing liquid 4# contains a higher concentration of Te, which is to be recovered. The process is as follows:

[0052] (1) Concentration stage

[0053] The amount of chlorine-containing liquid 4# is large and the chloride ion concentration is very low. After mixing, the chloride ion concentration obviously does not reach 100g / L. Therefore, it is concentrated. First, JK206 type (Shanghai Nankai Resin Co., Ltd.) strong alkaline styrene anion exchange resin is used for adsorption and desorption (1.3L, 5wt% NaOH solution is added for desorption) to obtain 1.3L of concentrated liquid, and then evaporated and concentrated to 200mL to obtain about 101L of dechlorinated liquid that is basically free of chlorine, and about 200mL of enriched liquid, the main component of which is NaCl. The relevant results are shown in the table below.

[0054]

[0055] Note: The unit of each substance is g / L.

[0056] (2) Evaporation separation stage

[0057] The enriched liquid and chlorine-containing liquid 5# were processed twice. 100mL of enriched liquid, 100mL of chlorine-containing liquid 5# and the returned circulating liquid were added to a common evaporator and mixed. Sulfurous acid with a mass concentration of 5% was added. According to the Te concentration, about 40mL was required. Considering that the chlorine-containing liquid 5# may bring in unreacted sulfurous acid, it is difficult to detect accurately. In order to improve the grade of tellurium products and prevent excessive reagents from reducing too many impurities and unreacted reagents from entering the gas to affect the quality of hydrochloric acid, only 5mL was added here to prevent excessive, and the Te concentration in the residual liquid was detected, and an appropriate amount of reagents was added in the circulation stage. Since the acid / chlorine molar ratio is 0.8, which is less than 1, 15mL of commercially available 98% concentrated sulfuric acid was added to make the acid / chlorine molar ratio about 1.2, and then heated and distilled, the residual liquid volume was controlled at about 50mL, and the steam was condensed to obtain hydrochloric acid.

[0058] (3) Precious metal recovery stage

[0059] The residual liquid obtained in stage (2) is separated by sedimentation to obtain precious metal slurry and supernatant. There is no obvious stratification in the lower part of the precious metal slurry, which is directly centrifuged to obtain filtrate and solid. The solid is dissolved and crystallized using dilute hydrochloric acid prepared with dechlorination liquid at about 30°C to obtain sodium sulfate solution and 99.5% refined tellurium (precious slag).

[0060] (4) Cycle stage

[0061] The supernatant of step (3) and the centrifuged liquid are mixed, and the remaining Te in the sodium sulfite reduction solution is added slowly until almost no black matter is produced. A total of 0.8 g is added here, and filtered to obtain 95% crude tellurium. About 30 mL of the filtrate is returned to the evaporation separation stage as a circulating liquid.

[0062] The sodium sulfate solution obtained in stage (3) is circulated for dissolution and crystallization.

[0063] Repeat (2) to (4) to process the remaining enriched liquid and chlorine-containing liquid 5#, and obtain about 400 mL of hydrochloric acid, 1.2 g of refined tellurium (precious slag), about 100 mL of concentrated sodium sulfate solution, and 2.0 g of crude tellurium. The relevant results are as follows.

[0064]

[0065] Note: The unit of each substance is g / L.

[0066] The concentrated sodium sulfate solution is cooled to about 10°C for crystallization, and the mother liquor of the sodium sulfate crystals is filtered out and recycled as a solvent.

[0067] Embodiment 3:

[0068] There are two liquids that need to be processed: 1L chlorine-containing liquid 6# and 500mL chlorine-containing liquid 7#. Chlorine-containing liquid 6# contains extremely low concentrations of precious metals Pt and Rh, and it is difficult to recover the original liquid. The process is as follows:

[0069] (1) Concentration stage

[0070] After the two liquids are mixed, the chloride ion concentration is about 112g / L, which is greater than 100g / L. However, the chloride ion concentration of the larger volume of chlorine-containing liquid 6# is lower than 100g / L, and the acidity is not high, with an acid / chlorine molar ratio of only about 0.5. In order to increase the final hydrochloric acid concentration, it is further concentrated. 1L of chlorine-containing liquid 6# is evaporated and concentrated to a volume of about 400mL, and the evaporated gas is condensed and recovered to obtain a dechlorinated liquid with a chloride ion content of about 1g / L. The relevant results are shown in the table below.

[0071]

[0072] Note: The unit of Pt and Rh is g / m 3 , The rest of the units are g / L.

[0073] (2) Evaporation separation stage

[0074] Since the acid / chlorine molar ratio after the two liquids are mixed is about 0.7, which is less than 1, 145 mL of commercially available 98% sulfuric acid is added to increase the acid / chlorine molar ratio to about 1.8. The chlorine-containing liquid 6# contains a small amount of sodium sulfite, a reagent, and no additional reagent is added here. The enriched liquid, chlorine-containing liquid 7# and the returned circulating liquid are added to a common evaporator for heating and distillation, and the residual liquid volume is controlled to be about 300 mL. The steam is condensed and recovered to obtain hydrochloric acid.

[0075] (3) Precious metal recovery stage

[0076] The residual liquid obtained in stage (2) is separated by sedimentation to obtain precious metal slurry and supernatant. There is no obvious stratification in the lower part of the precious metal slurry, which is directly centrifuged to obtain filtrate and solid. The solid is slurried with dechlorination liquid to dissolve the soluble crystals, and the precious slag in powder and needle-shaped crystals is obtained by filtration.

[0077] (4) Cycle stage

[0078] About 60 mL of the solution obtained by slurry mixing in stage (3) is cooled to about 10°C for crystallization, and the crystallization mother liquor of the salt crystals is filtered out and recycled as a solvent for precious metal layer treatment. The supernatant of step (3) and the centrifuged separation liquid are mixed to about 280 mL. Since there are fewer impurities, it can be directly returned. If the soluble silicate accumulates after a large number of cycles (about 0.1 g / L is brought into the wastewater), resulting in a significant increase in the viscosity of the liquid, CaO is added to the theoretical amount of silicate to react for purification treatment, which can remove part of the silicate that affects the viscosity of the liquid. It is also possible to separate part of the liquid for treatment each time to achieve the same effect. A small amount of purified slag and purified liquid are obtained by filtration. The main component of the purified slag is calcium sulfate, which can be recycled. The purified liquid is incorporated into the supernatant and the whole is returned to the evaporation separation stage as a circulating liquid.

[0079] After steps (1) to (4), a total of 700 mL of hydrochloric acid and 4.5 g of precious slag were obtained, the main components of which were lead sulfate and calcium sulfate. The total grade of rhodium and platinum was about 500 g / t. The relevant results are shown in the table below.

[0080]

[0081] Note: The unit of each substance is g / L.

[0082] The above implementation cases are only used to illustrate the preferred implementation modes of the present invention, but the present invention is not limited to the above implementation modes. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention within the scope of knowledge possessed by ordinary technicians in the field shall be deemed to be within the scope of protection of this application.

Claims

1. A process for treating high-chloride materials in precious metal smelting, characterized in that: The steps include: (1) Concentration When the total soluble chlorine in the mixed liquid of the chlorine-containing materials to be treated is above 100g / L, this stage can be skipped. When the total soluble chlorine in the mixed liquid of the chlorine-containing materials to be treated is less than 100g / L or even when the total soluble chlorine in the mixed liquid of the chlorine-containing materials to be treated is above 100g / L, the following operations are performed for the chlorine-containing liquid in which the chloride ion concentration is lower than 100g / L: a. Sort the chlorine-containing liquids with chloride ion concentrations lower than 100g / L by acidity, and use the lowest one or several as chlorine-containing liquid A, and the rest as chlorine-containing materials B; b. Separating and enriching the chloride ions in the chlorine-containing liquid A to obtain an enriched liquid C and a dechlorinated liquid D; (2) Evaporation separation The chlorine-containing substance B, the enriched liquid C and the circulating liquid H are sent to the evaporation crystallization device for mixing, and then the reagent E is added in an amount not higher than the theoretical required amount according to the amount of precious metals to be recovered in the mixed liquid. If the acid / chlorine molar ratio after mixing is less than 1, the reagent F is added to make the acid / chlorine molar ratio 1-3, otherwise it is not necessary to add; the mixed liquid is heated and evaporated, and hydrochloric acid is obtained after the steam is condensed; If the wastewater to be treated contains selenium, the hydrochloric acid is used for liquid-solid separation to obtain crude selenium solid; the remaining non-volatile matter forms residual liquid at the bottom of the distillation device; (3) Precious metal recovery The residual liquid obtained in step (2) is subjected to sedimentation separation to obtain a supernatant and a precious metal slurry, the precious metal slurry is centrifuged, the filtrate is merged into the supernatant, the solid layer containing salt crystals is added with a dechlorination liquid D, stirred and dissolved, and then filtered to obtain a precious residue and a concentrated salt solution; (4) Circulation Concentrated salt solution circulation: The concentrated salt solution is circulated as a solvent to dissolve salt crystals. When it reaches a certain concentration, it is concentrated, cooled and crystallized. After the salt crystals are separated, the crystallization mother liquor is continuously circulated as a solvent. When the chloride ion concentration in the crystallization mother liquor reaches 100g / L or above, it is incorporated into the supernatant for treatment; Supernatant liquid circulation: a portion or all of the obtained supernatant liquid is separated and added to reagent G for purification, and the qualified circulating liquid H is returned to step (2). If the process produces purified slag containing valuable elements, the purified slag can be recycled as concentrate.

2. The process for treating high-chloride materials for precious metal smelting according to claim 1, characterized in that: In step (1), the chlorine-containing material is a liquid or solid in which chlorine is in a -1 valence form or in a -1 valence form after mixed treatment.

3. The process for treating high-chloride materials for precious metal smelting according to claim 1, characterized in that: In step (1), the precious metal in the chlorine-containing material is one or more of Au, Ag, Se, Cu, Te, Pt, Pd, and Rh.

4. The process for treating high-chloride materials for precious metal smelting according to claim 1, characterized in that: In step (1), separation and enrichment of chloride ions in the chlorine-containing liquid A refers to separation and enrichment of chloride ions in the chlorine-containing liquid A by one or more of conventional evaporation concentration, ion exchange and membrane separation methods.

5. The process for treating high-chloride materials for precious metal smelting according to claim 1, characterized in that: In step (2), the evaporation crystallization device is one or a combination of an OSLO type crystallizer, a DTB type crystallizer, a common evaporator and a reactor.

6. The process for treating high-chloride materials for precious metal smelting according to claim 1, characterized in that: In step (2), the reagent E is one or more of sulfurous acid, sodium chloride, sodium thiosulfate, sodium sulfite, a metal element and hydrazine hydrate, and the added amount is 0.1 to 0.9 times the theoretically required amount.

7. The process for treating high-chloride materials for precious metal smelting according to claim 1, characterized in that: In step (2), the reagent F is one or a mixture of several of sulfuric acid, phosphoric acid, hydrochloric acid, hydrobromic acid, nitric acid and sulfurous acid.

8. The process for treating high-chloride materials for precious metal smelting according to claim 1, characterized in that: In step (4), the reagent G is a mixture of one or more of calcium carbonate, calcium oxide, sodium hydroxide, magnesium oxide, and sodium sulfide. The minimum amount of reagent G added is the theoretical reaction amount required for the difference between the impurities in the supernatant and the circulating fluid added in stage (2). The maximum amount of reagent G added is 0.8 times the amount required for the theoretical reaction of the impurities in the supernatant.

Citation Information

Patent Citations

  • System and method for treating metal chloride wastewater

    CN108164074A

  • Method for comprehensively recovering multiple elements and enriching gold and silver noble metals of steel ash

    CN110184471A

  • Method for recovering noble metals

    CN114555840A

  • Method for recovering noble metal

    JP2021123791A

  • Method and apparatus for the recovery and deep treatment of polluted acid

    US20190023585A1