Modified lepidolite slag artificial lightweight aggregate and preparation method thereof

Through the preparation method of modified lithium mica slag artificial light aggregate, the combination of lithium slag and other raw materials and the modification treatment, the problems of lithium slag resource utilization and light aggregate performance improvement are solved, and efficient resource recycling and Performance improvement.

CN118878232APending Publication Date: 2024-11-01JIANGXI BUILDING MATERIALS RES & DESIGN INST CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410945554.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The lithium slag resources generated by the lithium battery industry have not been effectively utilized, resulting in waste of resources and environmental pollution. The existing light aggregate preparation process has problems such as high amount of binder and difficulty in adjusting performance.

Method used

Use modified lithium mica slag artificial light aggregates, mix lithium slag with finely ground lithium slag, silicone materials, binders and other raw materials in a specific proportion, and undergo granulation, pre-curing and autoclaving treatment, and finally The surface is sprayed with a modifier to form a hydrophobic film, and an extrusion granulation process is used to increase density and strength.

Benefits of technology

Effectively utilize lithium mica slag resources, reduce production costs, improve the stacking density, water absorption and cylinder pressure strength of light aggregates, form a hydrophobic surface, extend service life, save binder usage, and improve production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004945516570000031
    Figure BDA0004945516570000031
  • Figure HDA0004945516590000011
    Figure HDA0004945516590000011
  • Figure HDA0004945516590000012
    Figure HDA0004945516590000012
Patent Text Reader

Abstract

The invention discloses a modified lepidolite slag artificial lightweight aggregate and a preparation method thereof, and belongs to the technical field of solid waste treatment and resource utilization, the modified lepidolite slag artificial lightweight aggregate comprises the following raw materials by mass: 30-60% of lithium slag, 15-20% of ground lithium slag, 10-20% of a siliceous material, 8-10% of a binder, and an activator accounting for 0-0.2% of the total mass of the binder, the water accounts for 3-5% of the total mass of the raw materials, and the modifier accounts for 5-10% of The lithium slag generated by lepidolite mineral separation is used as a main raw material, the raw materials are uniformly mixed through raw material grain composition optimization, and the artificial lightweight aggregate with the bulk density of 900-1200kg / m < 3 >, the 1h water absorption rate of less than 10% and the cylinder compressive strength of 4.0-13.0 MPa can be obtained through the processes of watering stirring, compaction granulation, demolding maintenance, interface modification and the like. The artificial lightweight aggregate prepared by the invention can be used for industrial products such as light bricks, light concrete, light prefabricated parts and the like, and resource utilization of the lepidolite slag is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid waste treatment and resource utilization, and specifically relates to a modified lepidolite slag artificial lightweight aggregate and a preparation method thereof. Background Art

[0002] With the rapid development of the lithium battery industry, a large amount of lithium slag is produced during lithium mining and lithium battery production. These lithium slags contain rich elements such as silicon, aluminum, and calcium. Direct disposal not only causes a waste of resources, but also causes serious environmental pollution. Therefore, how to effectively utilize lithium slag and turn waste into treasure has important environmental and economic significance.

[0003] In addition to the advantages of ordinary concrete such as firmness, durability, and formability, lightweight aggregate concrete prepared from artificial lightweight aggregate also has the advantage of being lightweight (it can reduce its own weight by 20% to 30% compared to ordinary concrete), and can change its strength, thermal properties and other properties with changes in density. It can be used in building structures, enclosures, thermal insulation, lightweight filling, prefabricated components, floating buildings and other fields. Summary of the invention

[0004] In order to solve the above problems, the present invention adopts the following technical solutions:

[0005] A modified lithium mica slag artificial lightweight aggregate comprises the following raw materials in percentage by mass: the raw materials comprise 30-60% lithium slag, 15-20% ground lithium slag, 10-20% siliceous material, and 8-10% binder.

[0006] The invention also comprises an activator accounting for 0 to 0.2% of the total mass of the binder, water accounting for 3 to 5% of the total mass of the raw materials, and a modifier accounting for 5 to 10% of the total mass of the raw materials.

[0007] Preferably, the particle size of the lithium slag is between 30 and 80 meshes, the moisture content is less than 15%, and the specific surface area of ​​the ground lithium slag is 450 to 600 m 2 / kg.

[0008] Preferably, the SiO2 content of the siliceous material is greater than 70%.

[0009] Preferably, the siliceous material is one or more high-silicon tailings such as copper tailings, tungsten tailings, molybdenum tailings and iron tailings.

[0010] Preferably, the binder is one or more of cement, fly ash, mineral powder, quicklime, gypsum and steel slag, and the activator is one or more of triethanolamine, triisopropanolamine, water glass and sodium sulfate.

[0011] Preferably, the modifier is one or more of sodium methyl silicate, polymethyltriethoxysilane, polyvinyl alcohol and alkyl phenyl sulfonate.

[0012] Preferably, the binder contains cement and / or quicklime, wherein the cement content is ≤40wt% and the quicklime content is ≤20wt%.

[0013] The present invention also discloses a method for preparing modified lepidolite slag artificial lightweight aggregate, comprising the following steps:

[0014] S1: mixing lithium slag and ground lithium slag evenly according to the proportion, adding a binder, mixing evenly, and finally adding an aqueous solution containing an activator and mixing until evenly mixed to obtain a mixed material;

[0015] S2: Weigh the mixed material and granulate it to obtain a ball with a smooth surface;

[0016] S3: Pre-curing the balls and then autoclaving them to obtain lightweight aggregates

[0017] S4: Atomize the modifier and spray it evenly on the surface of the rotating light aggregate. After standing for 1 to 2 hours, the modified lithium mica slag artificial light aggregate is obtained.

[0018] Preferably, in step S2,

[0019] The granulation is specifically as follows: the mixture material is placed in a double-roll granulator, the loading pressure is 1.0-3.0 kN, and the loading speed is 50-200 rpm to pass through a die with a particle size of 3-10 mm.

[0020] Preferably, in step S3,

[0021] Pre-curing is as follows: placing the pellets in a sealed state at 25-30°C for 8-12 hours;

[0022] The autoclave curing is specifically as follows: the pre-cured pellets are placed in an autoclave and cured for 12 to 24 hours under curing conditions with a carbon dioxide concentration of 80 to 90%, a pressure of 0.8 to 1.2 MPa, a temperature of 80 to 100° C., and a humidity of 65 to 80%.

[0023] Beneficial effects of the present invention:

[0024] (1) The present invention effectively utilizes lithium mica slag resources, reduces waste discharge and storage problems, reduces production costs, and complies with the concept of resource recycling.

[0025] (2) The bulk density of the modified lithium mica slag artificial lightweight aggregate provided by the present invention is less than 1200 kg / m 3 , 1h water absorption rate is less than 10%, and the cylinder pressure strength can reach up to 13.0MPa.

[0026] (3) The surface of the modified lithium mica slag artificial lightweight aggregate of the present invention is specially treated to form a hydrophobic film on the surface thereof, which has a low water absorption rate and can effectively prevent water intrusion and improve durability.

[0027] (4) The modified lithium mica slag artificial lightweight aggregate of the present invention is granulated by extrusion, which requires less binder, is easy to adjust parameters, has high production efficiency, and saves energy. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a flow chart for preparing the modified lepidolite artificial lightweight aggregate.

[0029] Figure 2 This is a physical picture of the modified lepidolite artificial lightweight aggregate prepared in Example 1 of the present invention.

[0030] Figure 3 This is a SEM image of the modified lepidolite artificial lightweight aggregate prepared in Example 1 of the present invention.

[0031] Figure 4 This is a SEM image of the modified lepidolite artificial lightweight aggregate prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The lithium slag used in the embodiment of the present invention is taken from Fengxin County, Jiangxi Province. The chemical composition of the lithium slag and the main raw materials is shown in Table 1. The lithium slag is mainly composed of calcium feldspar, gypsum and quartz, which can be used as a calcium raw material, and the tungsten tailings are mainly composed of quartz, which can be used as a silicon raw material.

[0033] Table 1 Chemical composition of raw materials

[0034]

[0035] The lithium slag used in the present invention is directly taken from the manufacturer. Since the lithium slag has the characteristics of coarse particle size and high water content, it is not conducive to sufficient stirring. By utilizing its good grindability, part of the lithium slag can be dried, ground and mixed into the lithium slag to adjust the gradation and facilitate stirring. At the same time, the double-roll extrusion method can make the lithium slag fully contact with other raw materials to produce hydration reaction, further make the aggregate dense and improve the cylinder pressure strength, and reduce the production cost.

[0036] Preparation process reference Figure 1 , the actual picture obtained is referenced Figure 2 .

[0037] Embodiment 1:

[0038] (1) Weighing raw materials of lithium slag, ground lithium slag, siliceous material and binder in a mass ratio of 50:20:10:20; wherein the siliceous material is tungsten tailings, and the mass ratios of cement, fly ash, mineral powder and quicklime in the binder are 10:3:2:5 respectively; the activator is triethanolamine, and the modifier is sodium methyl silicate;

[0039] (2) lithium slag and ground lithium slag are placed in a mixer according to the proportion and stirred for 6 minutes until they are uniformly mixed, fly ash, mineral powder, cement, and quicklime are added in sequence and stirred for 3 minutes until they are uniformly mixed, and finally an aqueous solution containing an activator is added and stirred for 3 minutes until they are uniformly mixed;

[0040] (3) Weigh an appropriate amount of the prepared mixed material and add it to a double-roll granulator, adjust the loading pressure to 3.0 kN, and pass it through a die with a particle size of 5 mm at a loading speed of 100 rpm to obtain a ball with a smooth surface;

[0041] (4) The prepared pellets are sealed and pre-cured at 25° C. for 12 h, and then the pre-cured pellets are placed in an autoclave and cured for 24 h under curing conditions of 90 vt% carbon dioxide concentration, 1.0 MPa pressure, 80° C. temperature, and 80% humidity to obtain lightweight aggregate;

[0042] (5) The light aggregate is taken out and placed on a turntable, and a 20 wt% sodium methyl silicate solution is atomized and evenly sprayed on the surface of the rotating material ball. After standing for 1 hour, the modified lithium mica slag artificial light aggregate is obtained.

[0043] After testing, the bulk density of the modified lithium mica slag artificial lightweight aggregate prepared in this embodiment is 1180kg / m 3 , 1h water absorption rate is 4.6%, and cylinder pressure strength is 12.8MPa.

[0044] Comparative Example 1:

[0045] (1) Weighing raw materials of lithium slag, ground lithium slag, siliceous material and binder in a mass ratio of 45:15:10:30; wherein the siliceous material is tungsten tailings, and the mass ratios of cement, fly ash, mineral powder and quicklime in the binder are 10:3:2:5 respectively; the activator is triethanolamine, and the modifier is sodium methyl silicate;

[0046] (2) lithium slag and ground lithium slag are placed in a mixer according to the proportion and stirred for 6 minutes until they are uniformly mixed, fly ash, mineral powder, cement, and quicklime are added in sequence and stirred for 3 minutes until they are uniformly mixed, and finally an aqueous solution containing an activator is added and stirred for 3 minutes until they are uniformly mixed;

[0047] (3) Weigh an appropriate amount of the prepared mixed material and add it to a granulating disc machine and rotate it at 60 rpm until a smooth ball with a particle size of about 5 mm is formed;

[0048] (4) The prepared pellets are sealed and pre-cured at 25° C. for 12 h, and then the pre-cured pellets are placed in an autoclave and cured for 24 h under curing conditions of 90 vt% carbon dioxide concentration, 1.0 MPa pressure, 80° C. temperature, and 80% humidity to obtain lightweight aggregate;

[0049] (5) The light aggregate is taken out and placed on a turntable, and a 20 wt% sodium methyl silicate solution is atomized and evenly sprayed on the surface of the rotating material ball. After standing for 1 hour, the modified lithium mica slag artificial light aggregate is obtained.

[0050] After testing, the bulk density of the modified lithium mica slag artificial lightweight aggregate prepared in this embodiment is 920kg / m 3 , 1h water absorption rate is 8.1%, and cylinder pressure strength is 6.2MPa.

[0051] Comparative Example 2:

[0052] (1) Weighing raw materials with a mass ratio of lithium slag, siliceous material and binder of 70:10:20; wherein the siliceous material is tungsten tailings, and the mass ratios of cement, fly ash, mineral powder and quicklime in the binder are 10:3:2:5 respectively; the activator is triethanolamine, and the modifier is sodium methyl silicate;

[0053] (2) according to the proportion, the lithium slag is placed in a mixer and stirred for 6 minutes, fly ash, mineral powder, cement, and quicklime are added in sequence and mixed and stirred for 3 minutes until uniform, and finally, an aqueous solution containing an activator is added and stirred for 3 minutes until uniform;

[0054] (3) Weigh an appropriate amount of the prepared mixed material and add it to a double-roll granulator, adjust the loading pressure to 3.0 kN, and pass it through a die with a particle size of 5 mm at a loading speed of 100 rpm to obtain a ball with a smooth surface;

[0055] (4) The prepared pellets are sealed and pre-cured at 25° C. for 12 h, and then the pre-cured pellets are placed in an autoclave and cured for 24 h under curing conditions of 90 vt% carbon dioxide concentration, 1.0 MPa pressure, 80° C. temperature, and 80% humidity to obtain lightweight aggregate;

[0056] (5) The light aggregate is taken out and placed on a turntable, and a 20 wt% sodium methyl silicate solution is atomized and evenly sprayed on the surface of the rotating material ball. After standing for 1 hour, the modified lithium mica slag artificial light aggregate is obtained.

[0057] After testing, the bulk density of the modified lithium mica slag artificial lightweight aggregate prepared in this embodiment is 1020kg / m 3 , 1h water absorption rate is 6.3% and cylinder pressure strength is 8.8MPa.

[0058] Comparative Example 3:

[0059] (1) Weighing raw materials of lithium slag, ground lithium slag, siliceous material and binder in a mass ratio of 50:20:10:20; wherein the siliceous material is tungsten tailings, and the mass ratios of cement, fly ash, mineral powder and quicklime in the binder are 10:3:2:5 respectively; the activator is triethanolamine, and the modifier is sodium methyl silicate;

[0060] (2) lithium slag and ground lithium slag are placed in a mixer according to the proportion and stirred for 6 minutes until they are uniformly mixed, fly ash, mineral powder, cement, and quicklime are added in sequence and stirred for 3 minutes until they are uniformly mixed, and finally an aqueous solution containing an activator is added and stirred for 3 minutes until they are uniformly mixed;

[0061] (3) Weigh an appropriate amount of the prepared mixed material and add it to a double-roll granulator, adjust the loading pressure to 3.0 kN, and pass it through a die with a particle size of 5 mm at a loading speed of 100 rpm to obtain a ball with a smooth surface;

[0062] (4) The prepared pellets are sealed and pre-cured at 25°C for 12 hours, and then the pre-cured pellets are placed in an autoclave and cured for 24 hours at a carbon dioxide concentration of 90vt%, a pressure of 1.0MPa, a temperature of 80°C, and a humidity of 80% to obtain artificial lightweight aggregate.

[0063] After testing, the bulk density of the modified lithium mica slag artificial lightweight aggregate prepared in this embodiment is 1130kg / m 3 , 1h water absorption rate is 9.3%, and cylinder pressure strength is 12.2MPa.

[0064] Embodiment 2:

[0065] (1) Weighing raw materials of lithium slag, ground lithium slag, siliceous material and binder in a mass ratio of 50:20:10:20; wherein the siliceous material is tungsten tailings, and the mass ratios of cement, fly ash, mineral powder and quicklime in the binder are 10:3:2:5 respectively; the activator is triethanolamine, and the modifier is sodium methyl silicate;

[0066] (2) lithium slag and ground lithium slag are placed in a mixer according to the proportion and stirred for 6 minutes until they are uniformly mixed, fly ash, mineral powder, cement, and quicklime are added in sequence and stirred for 3 minutes until they are uniformly mixed, and finally an aqueous solution containing an activator is added and stirred for 3 minutes until they are uniformly mixed;

[0067] (3) Weigh an appropriate amount of the prepared mixed material and add it to a roller granulator, adjust the loading pressure to 1.0 kN, and pass it through a die with a particle size of 5 mm at a loading speed of 50 rpm to obtain a ball with a smooth surface;

[0068] (4) The prepared pellets are sealed and pre-cured at 25° C. for 12 h, and then the pre-cured pellets are placed in an autoclave and cured for 24 h under curing conditions of 90 vt% carbon dioxide concentration, 1.0 MPa pressure, 80° C. temperature, and 80% humidity to obtain lightweight aggregate;

[0069] (5) The light aggregate is taken out and placed on a turntable, and a 20 wt% sodium methyl silicate solution is atomized and evenly sprayed on the surface of the rotating material ball. After standing for 1 hour, the modified lithium mica slag artificial light aggregate is obtained.

[0070] After testing, the bulk density of the modified lithium mica slag artificial lightweight aggregate prepared in this embodiment is 910kg / m 3 , 1h water absorption rate is 5.3% and cylinder pressure strength is 7.7MPa.

[0071] Embodiment 3:

[0072] (1) Weighing raw materials with a mass ratio of 60:20:10:10 among lithium slag, ground lithium slag, siliceous material and binder; wherein the siliceous material is tungsten tailings, and the mass ratios of cement, fly ash, mineral powder and quicklime in the binder are 8:5:3:4 respectively; the activator is triethanolamine, and the modifier is sodium methyl silicate;

[0073] (2) lithium slag and ground lithium slag are placed in a mixer according to the proportion and stirred for 6 minutes until they are uniformly mixed, fly ash, mineral powder, cement, and quicklime are added in sequence and stirred for 3 minutes until they are uniformly mixed, and finally an aqueous solution containing an activator is added and stirred for 3 minutes until they are uniformly mixed;

[0074] (3) Weigh an appropriate amount of the prepared mixed material and add it to a double-roll granulator, adjust the loading pressure to 3.0 kN, and pass it through a die with a particle size of 5 mm at a loading speed of 100 rpm to obtain a ball with a smooth surface;

[0075] (4) The prepared pellets are sealed and pre-cured at 25° C. for 12 h, and then the pre-cured pellets are placed in an autoclave and cured for 24 h under curing conditions of 90 vt% carbon dioxide concentration, 1.0 MPa pressure, 80° C. temperature, and 80% humidity to obtain lightweight aggregate;

[0076] (5) The light aggregate is taken out and placed on a turntable, and a 20 wt% sodium methyl silicate solution is atomized and evenly sprayed on the surface of the rotating material ball. After standing for 1 hour, the modified lithium mica slag artificial light aggregate is obtained.

[0077] After testing, the bulk density of the modified lithium mica slag artificial lightweight aggregate prepared in this embodiment is 1160kg / m 3 , 1h water absorption rate is 4.9%, and cylinder pressure strength is 10.2MPa.

[0078] By comparing the above Example 1 and Comparative Example 1, it can be seen that the present invention improves the granulation method to extrusion granulation, so that the lithium slag can fully contact with other raw materials for hydration reaction, thereby significantly improving the performance of the lightweight aggregate with less binder dosage.

[0079] At the same time, the modified lithium mica artificial light aggregates prepared in Example 1 and Comparative Example 1 were scanned by electron microscope, and the results are shown in Figure 3 and 4 ,from Figure 3It can be seen that the interior of the lightweight aggregate prepared in the embodiment is a relatively dense whole with fewer pores and abundant hydration products; the lightweight aggregate prepared in comparative example 1 has more pores inside and the pores are of different sizes, and some fly ash particles do not participate in hydration; it also further illustrates that the present invention improves the granulation method into extrusion granulation, so that the lithium slag can fully contact with other raw materials for hydration reaction, thereby significantly improving the performance of the lightweight aggregate with less binder dosage.

[0080] By comparing Example 1 and Comparative Example 2, it can be seen that since lithium slag has the characteristics of coarse particle size and high water content, it is not conducive to sufficient stirring. By utilizing its good grindability, part of the lithium slag can be dried and ground and mixed into the lithium slag to adjust the grading and facilitate stirring, thereby improving the performance of the lightweight aggregate.

[0081] By comparing Example 1 and Comparative Example 3, it can be seen that the present invention sprays a modifier on the surface of the light aggregate after curing to form a hydrophobic film on the surface to prevent water intrusion and greatly reduce the water absorption rate.

[0082] By comparing Examples 1-3, it can be seen that the present invention adopts appropriate loading pressure to ensure the performance of the lightweight aggregate, while the pressure adopted in Comparative Example 4 is too small, resulting in insufficient contact, which affects the hydration reaction of the lightweight aggregate and causes poor performance.

[0083] The above is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. It is not necessary and impossible to list all implementation methods here, so any slight modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still belongs to the scope of the technical solution of the present invention.

Claims

1. A modified lepidolite slag artificial lightweight aggregate, characterized in that: The raw materials include the following percentages by mass: 30-60% lithium slag, 15-20% ground lithium slag, 10-20% siliceous material, and 8-10% binder. The invention also comprises an activator accounting for 0 to 0.2% of the total mass of the binder, water accounting for 3 to 5% of the total mass of the raw materials, and a modifier accounting for 5 to 10% of the total mass of the raw materials.

2. The modified lepidolite slag artificial lightweight aggregate according to claim 1, characterized in that: The particle size of the lithium slag is between 30 and 80 meshes, the moisture content is less than 15%, and the specific surface area of ​​the ground lithium slag is 450 to 600 m 2 / kg.

3. The modified lepidolite slag artificial lightweight aggregate according to claim 1, characterized in that: The SiO2 content of the siliceous material is greater than 70%.

4. The modified lepidolite slag artificial lightweight aggregate according to claim 1, characterized in that: The siliceous material is one or more of high-silicon tailings such as copper tailings, tungsten tailings, molybdenum tailings and iron tailings.

5. The modified lepidolite slag artificial lightweight aggregate according to claim 1, characterized in that: The binder is one or more of cement, fly ash, mineral powder, quicklime, gypsum and steel slag, and the activator is one or more of triethanolamine, triisopropanolamine, water glass and sodium sulfate.

6. The modified lepidolite slag artificial lightweight aggregate according to claim 1, characterized in that: The modifier is one or more of sodium methyl silicate, polymethyltriethoxysilane, polyvinyl alcohol and alkyl phenyl sulfonate.

7. The modified lepidolite slag artificial lightweight aggregate according to claim 4, characterized in that: The binder contains cement and / or quicklime, wherein the cement content is ≤40wt% and the quicklime content is ≤20wt%.

8. The method for preparing the modified lepidolite slag artificial lightweight aggregate according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: mixing lithium slag and ground lithium slag evenly according to the proportion, adding a binder, mixing evenly, and finally adding an aqueous solution containing an activator and mixing until evenly mixed to obtain a mixed material; S2: Weigh the mixed material and granulate it to obtain a ball with a smooth surface; S3: pre-curing the material balls and then autoclaving them to obtain lightweight aggregates; S4: Atomize the modifier and spray it evenly on the surface of the rotating light aggregate. After standing for 1 to 2 hours, the modified lithium mica slag artificial light aggregate is obtained.

9. The preparation method according to claim 8, characterized in that: In step S2, The granulation is specifically as follows: the mixture material is placed in a double-roll granulator, the loading pressure is 1.0-3.0 kN, and the loading speed is 50-200 rpm to pass through a die with a particle size of 3-10 mm.

10. The preparation method according to claim 8, characterized in that: In step S3, Pre-curing is as follows: placing the pellets in a sealed state at 25-30°C for 8-12 hours; The autoclave curing is specifically as follows: the pre-cured pellets are placed in an autoclave and cured for 12 to 24 hours under curing conditions with a carbon dioxide concentration of 80 to 90%, a pressure of 0.8 to 1.2 MPa, a temperature of 80 to 100° C., and a humidity of 65 to 80%.

Citation Information

Cited By

  • Lithium slag-based unfired lightweight aggregate and preparation method thereof

    CN119080414A

  • A non-fired lightweight aggregate with high lithium slag content and a method for its co-preparation using lepidolite slag and spodumene slag.

    CN120309273B

  • Mixed aggregate based on steel slag and lithium slag as well as preparation method and application of mixed aggregate

    CN120573971A