Low-carbon concrete and preparation method thereof
By using fly ash and modified recycled concrete aggregate in concrete, combined with self-healing materials, the problem of high carbon emissions of traditional concrete is solved, low carbon emissions and durability are improved, and it meets the requirements of sustainable development.
Patent Information
- Application Number
- CN202410973938.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Large amounts of carbon dioxide emissions in traditional concrete production have negative impacts on the environment, and low-carbon concrete needs to be developed to reduce carbon emissions.
Fly ash is used to replace cement, and by modifying regenerated concrete aggregates and self-healing materials, carbon emissions are reduced and the mechanical properties and durability of concrete are improved.
It significantly reduces carbon emissions, improves the durability and compressive strength of concrete, extends the service life of the structure, and conforms to the concept of sustainable development.
Smart Images

Figure BDA0004954002290000101 
Figure BDA0004954002290000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to low-carbon concrete and a preparation method thereof. Background Art
[0002] Concrete is one of the most basic and widely used building materials in modern construction. Concrete is widely used, from house construction to large infrastructure such as bridges, tunnels and dams. Its history can be traced back to ancient civilizations. The main components of concrete are cement, sand, gravel and water. It is mixed, poured and cured. It has excellent strength and durability and is suitable for various building structures and foundation projects. The main component of concrete is cement. Its preparation process requires a lot of energy, mainly coal or natural gas, which leads to a large amount of carbon dioxide (CO2) emissions in the concrete production process. Although cement will carbonize and partially absorb carbon dioxide during the curing process, its production stage is still one of the main sources of carbon emissions in the construction industry. Traditional concrete is widely used because of its high strength and durability. It can withstand heavy loads and long-term wind and rain, making it an ideal choice for large-scale infrastructure and construction projects.
[0003] Despite the outstanding performance of concrete in the construction field, its production and use also face some important problems. The large amount of carbon dioxide emissions during cement production has a negative impact on the environment, exacerbating global warming and climate change. Due to the large amount of heat required and the chemical reactions involved, the process of cement production produces about 4 billion tons of carbon dioxide each year, accounting for about 8% of global carbon dioxide emissions.
[0004] In order to solve the environmental problems of traditional concrete, it is necessary to develop a low-carbon concrete by reducing or replacing cement in traditional concrete, or by using alternative materials to reduce carbon emissions. Summary of the invention
[0005] The present invention aims to solve at least one of the above technical problems existing in the prior art. To this end, the present invention provides a low-carbon concrete, which significantly reduces carbon emissions by reducing the amount of cement used and using alternative materials such as fly ash.
[0006] The invention also provides a method for preparing low-carbon concrete.
[0007] A first aspect of the present invention provides a low-carbon concrete, wherein the raw materials for preparing the low-carbon concrete include cement, fly ash, modified recycled concrete aggregate, coarse sand and self-healing material.
[0008] One of the technical solutions of the present invention regarding low-carbon concrete has at least the following beneficial effects:
[0009] The low-carbon concrete of the present invention is a new material with the main goal of reducing carbon emissions. It significantly reduces carbon emissions by reducing the amount of cement used and using alternative materials such as fly ash. Carbon dioxide emissions during cement production are one of the main sources of greenhouse gases, and alternative materials such as fly ash can not only reduce dependence on natural resources, but also effectively reduce the carbon footprint of concrete production.
[0010] The low-carbon concrete of the present invention can improve its interface performance and bonding strength with cement matrix after the recycled concrete aggregate is modified, which not only effectively utilizes waste concrete resources, but also improves the mechanical properties and durability of concrete and prolongs the service life of the structure.
[0011] The addition of coarse sand can improve the working performance and compressive strength of concrete, while ensuring the fluidity and compactness of concrete.
[0012] The self-healing materials added to low-carbon concrete can fill and repair cracks after micro-cracks in the concrete occur, thereby delaying and preventing the expansion of cracks and improving the durability and maintenance cost of concrete.
[0013] Since low-carbon concrete uses environmentally friendly raw materials and technologies in its preparation process, it reduces the consumption of natural resources and the impact on the environment. At the same time, since it improves the durability of concrete and reduces maintenance requirements, it can reduce the overall carbon footprint and life cycle costs, which is in line with the concept of sustainable development.
[0014] According to some embodiments of the present invention, the cement may be ordinary Portland cement.
[0015] According to some embodiments of the present invention, the preparation raw materials include, by weight:
[0016] Cement: 100 parts,
[0017] Fly ash: 10 to 30 parts,
[0018] Modified recycled concrete aggregate: 10 to 30 parts,
[0019] Coarse sand: 10 to 20 parts,
[0020] Self-healing material: 5 to 10 parts.
[0021] According to some embodiments of the present invention, the preparation raw materials include, by weight:
[0022] Cement: 100 parts,
[0023] Fly ash: 15 to 25 parts,
[0024] Modified recycled concrete aggregate: 15 to 25 parts,
[0025] Coarse sand: 10 to 20 parts,
[0026] Self-healing material: 5 to 10 parts.
[0027] According to some embodiments of the present invention, the method for preparing the modified recycled concrete aggregate is:
[0028] (1) soaking rubber powder in sodium hydroxide solution to obtain pretreated high-performance rubber powder;
[0029] (2) mixing the regenerated micropowder and the alkaline activator uniformly and then grinding them to obtain alkali-activated regenerated micropowder, wherein the alkaline activator is a mixture of magnesium hydroxide and trimethylamine in a mass ratio of 1 to 3:1;
[0030] (3) adding a silane coupling agent to the alkali-activated regenerated micropowder, stirring evenly, then adding polyvinyl alcohol, and continuing to stir to obtain pretreated regenerated micropowder;
[0031] (4) Mixing natural sand and gravel, the pretreated recycled fine powder and slag powder evenly to obtain the modified recycled concrete aggregate.
[0032] In step (1), the rubber powder is soaked in sodium hydroxide solution to obtain pretreated high-performance rubber powder. The sodium hydroxide solution can cause a chemical reaction on the surface of the rubber powder, improve its surface activity, and increase its bonding ability with the cement matrix. The pretreated rubber powder has better mechanical properties, such as tensile strength and elastic modulus, and can bear loads in concrete more effectively.
[0033] In step (2), the regenerated micropowder and the alkaline activator (a mixture of magnesium hydroxide and trimethylamine in a mass ratio of 1 to 3:1) are uniformly mixed and then ground to obtain alkali-activated regenerated micropowder. The mixture of magnesium hydroxide and trimethylamine can effectively activate the surface of the regenerated micropowder, improve its activity and bonding performance with the cement matrix. The alkaline activator helps to improve the dispersibility and uniformity of the regenerated micropowder, make it better in filling effect in concrete, reduce voids, and improve the density and strength of concrete.
[0034] The mixture of magnesium hydroxide and trimethylamine allows the system to have both strong alkalinity and weak alkalinity. These alkaline substances can provide some active sites on the surface of the micropowder. In an alkaline environment, the hydroxyl groups (-OH groups) on the surface of the micropowder are more likely to be in an activated state, which is conducive to subsequent surface chemical reactions. The mixed magnesium hydroxide and trimethylamine can increase the number of active sites on the surface of the micropowder, which can function more effectively when reacting with subsequently added chemical substances such as silane coupling agents. The mixed alkaline activator can interact with the minerals on the surface of the micropowder, change its surface charge state and chemical environment, and facilitate the subsequent coupling agent adsorption and intermolecular bonding. After activating the surface of the micropowder, its interaction with the cement matrix is enhanced, forming a stronger chemical bond structure, thereby improving the overall mechanical properties and durability of the modified recycled concrete aggregate.
[0035] In step (3), the silane coupling agent can form chemical bonds on the surface of the micropowder, enhance its bonding ability with the cement matrix, and reduce the generation of interface peeling and cracks. The addition of polyvinyl alcohol can improve the crack resistance and durability of concrete, help reduce the expansion of cracks in concrete, and extend the service life of the structure.
[0036] In step (4), natural sand and gravel provide the mechanical properties and durability required for concrete, and slag powder, as a supplementary material, can optimize the chemical properties and microstructure of concrete. The modified recycled concrete aggregate after uniform mixing combines the advantages of various raw materials, has good compressive strength, durability and self-healing ability, and can effectively meet the needs of different engineering applications.
[0037] According to some embodiments of the present invention, in step (1), the concentration of the sodium hydroxide solution is 10% to 20%.
[0038] Sodium hydroxide solution with a concentration lower than 10% may not be able to fully dissolve and activate the chemically reactive groups on the surface of the rubber powder, resulting in poor soaking effect and failure to achieve the expected surface modification effect. The insufficient surface activity of the rubber powder after soaking may lead to reduced bonding performance with the cement matrix, affecting the overall mechanical properties and durability of the modified concrete aggregate. Sodium hydroxide solution with too high a concentration is highly corrosive and may damage or over-activate the surface of the rubber powder, resulting in damage to the physical properties of the rubber powder or changes in its chemical properties. In addition, the use of high-concentration sodium hydroxide solution requires more energy to process and neutralize the remaining alkaline solution, increasing the energy consumption and cost of the production process. Therefore, 10% to 20% is a suitable concentration of sodium hydroxide solution.
[0039] According to some embodiments of the present invention, in step (1), the rubber powder may be waste rubber powder.
[0040] According to some embodiments of the present invention, in step (2), the mass ratio of the regenerated micropowder to the alkaline activator is 50:5-10.
[0041] At an appropriate mass ratio, the regenerated micropowder and alkaline activator can be mixed more evenly, ensuring that the formed alkali-activated regenerated micropowder particles are evenly distributed, which is conducive to the subsequent addition and dispersion of silane coupling agents and polyvinyl alcohol. Furthermore, an appropriate alkaline activator can increase the number of active sites on the surface of the regenerated micropowder and improve its bonding ability with the cement matrix. This helps to form a tighter chemical bond structure and enhance the strength and durability of concrete aggregates. In addition, an appropriate proportion of alkaline activators helps to optimize the microstructure of concrete, reduce the formation of pores and cracks, and thus improve the compressive strength and durability of concrete.
[0042] According to some embodiments of the invention, the self-healing material is a hollow polypropylene fiber.
[0043] Hollow polypropylene fibers can form a network structure inside concrete. When microcracks are formed in concrete under external forces, they can close these microcracks through water absorption and expansion or other mechanisms to prevent them from expanding and penetrating, thereby maintaining the structural integrity and durability of the concrete. When microcracks occur in concrete, hollow polypropylene fibers can prevent further expansion and propagation of cracks through their bending deformation or water absorption and expansion characteristics, thereby delaying the damage and aging process of the concrete structure. Hollow polypropylene fibers can also effectively reduce the risk of cracking and deterioration of concrete under harsh environmental conditions, thereby extending the service life and durability of concrete structures. The use of self-healing hollow polypropylene fibers can reduce the maintenance needs of concrete structures. By preventing the expansion of cracks and reducing the frequency of concrete repairs, maintenance costs and time costs are reduced.
[0044] Hollow polypropylene fibers generally have greater water absorption and expansion capacity than solid polypropylene fibers. When microcracks occur in concrete structures, hollow fibers can absorb and store water more effectively, thereby more effectively achieving automatic closure and repair of cracks. Since the interior of hollow fibers is a hollow structure, their density is generally lower than that of solid fibers of the same volume. This means that when hollow fibers are added to concrete, the overall density and weight of the concrete will not be significantly increased, which helps to maintain the lightweight characteristics of concrete. In addition, the microscopic network structure formed by hollow fibers in concrete can effectively improve the chemical resistance of concrete. This structure can prevent corrosive substances from invading the interior of concrete and slow down the aging of concrete structures. It can be understood that hollow fibers generally have better processing and dispersibility and can be more evenly distributed in concrete. This helps to improve the uniformity and engineering application performance of concrete and ensure the overall performance and stability of concrete structures. Since hollow fibers can effectively reduce cracks and damage in concrete structures, maintenance and repair costs can be reduced. This is particularly important for long-term infrastructure projects and can effectively extend the service life of the structure.
[0045] According to some embodiments of the present invention, the aspect ratio of the hollow polypropylene fiber is 10 to 20:1.
[0046] Hollow fibers with a larger aspect ratio generally have better water absorption and expansion capabilities and the ability to form a microscopic network. When microcracks occur in concrete structures, hollow fibers can absorb water more effectively and close the cracks by expanding, thereby achieving a self-healing effect. Fibers with a larger aspect ratio can more effectively control the expansion of cracks. The length of the fiber can span the cracks and effectively bridge them, preventing the cracks from further developing and deepening, thereby improving the crack resistance of concrete. In addition, fibers with a larger aspect ratio have better dispersion and uniformity in concrete, and will not have a significant adverse effect on the workability and fluidity of concrete. This helps to achieve uniform dispersion of fibers in concrete and improve the strength and durability of the overall concrete. Further, hollow fibers generally have a lighter density than solid fibers, despite their longer length. This helps to maintain the lightweight characteristics of concrete without significantly increasing the density and weight of concrete when adding fibers to concrete. As a result, hollow fibers with an appropriate aspect ratio can improve the durability and long-term performance of concrete. They can effectively prevent the formation and expansion of microcracks, reduce the maintenance requirements of concrete structures, and extend the service life of structures.
[0047] According to some embodiments of the present invention, the particle size of the coarse sand is 0.5 mm to 2.5 mm.
[0048] The appropriate particle size range of coarse sand helps improve the fluidity and workability of concrete. Larger particle sizes can fill larger voids in concrete without affecting the fluidity of concrete too much, which is beneficial for pouring and vibrating during construction. The appropriate particle size of coarse sand can enhance the compressive strength of concrete. This is because the larger particle size of coarse sand can form an effective inter-particle locking structure, increase the internal friction and compressive resistance of concrete, and thus improve the overall strength of concrete.
[0049] The second aspect of the present invention provides a method for preparing low-carbon concrete, which comprises: adding the cement, fly ash, modified recycled concrete aggregate and coarse sand into a mixing tank for stirring, and after mixing, adding the self-healing material until the self-healing material is evenly dispersed in the concrete slurry.
[0050] A technical solution in the method for preparing carbon concrete of the present invention has at least the following beneficial effects:
[0051] The preparation method of the present invention does not require expensive equipment and complicated process control, has undemanding reaction conditions, has readily available raw materials, has low production costs, and is easy to industrialize.
[0052] Using fly ash and modified recycled concrete aggregates to replace part of the cement can significantly reduce the carbon emissions of concrete. Fly ash is an industrial waste, and its use not only reduces dependence on natural resources, but also reduces CO2 emissions. Modified recycled concrete aggregates usually have excellent mechanical properties and anti-aging properties, which can effectively enhance the durability of concrete. These aggregates can reduce the propagation of cracks in concrete and reduce the shrinkage of concrete, thereby extending the service life of concrete structures.
[0053] The combination of modified recycled concrete aggregate and coarse sand can optimize the mechanical properties of concrete, such as compressive strength, flexural strength and freeze-thaw resistance. This combination can improve the overall quality and performance stability of concrete. The addition of self-healing materials can quickly release repair agents when micro-cracks occur in concrete, filling cracks and restoring the structural integrity of concrete. This self-healing ability can delay the aging and damage of concrete structures. The use of mixing tanks for mixing can ensure that various raw materials are fully and evenly mixed, thereby improving construction efficiency and project quality. The uniform dispersion of self-healing materials in the concrete paste can ensure its effectiveness and consistency in the entire concrete system.
[0054] According to some embodiments of the present invention, the method further comprises adjusting the water-cement ratio according to construction requirements after adding the self-healing material.
[0055] Adjusting the water-cement ratio can effectively control the fluidity and plasticity of concrete. After adding the self-healing material, increasing the water-cement ratio appropriately as needed can make the concrete easier to construct and vibrate, ensuring that the concrete can fully fill the mold and roller press during the pouring and molding process, thereby improving workability and construction efficiency. In addition, adjusting the water-cement ratio can help ensure the uniform dispersion of the self-healing material in the concrete paste. Appropriate adjustment of the water-cement ratio can make the fluidity and viscosity of the concrete paste reach the optimal state, which is conducive to the uniform distribution of the self-healing material inside the concrete, thereby ensuring its effective filling and repair ability at the microcracks of the concrete. Correctly adjusting the water-cement ratio can maximize the role of the self-healing material. Appropriately increasing the water-cement ratio can ensure that there is enough water in the concrete, promote the release and reaction of the active ingredients in the self-healing material, thereby accelerating the repair process of microcracks and maintaining the integrity and durability of the concrete structure. Finally, adjusting the water-cement ratio helps to improve the performance stability of concrete. By reasonably controlling the water-cement ratio, the porosity and sand shrinkage effect in the concrete can be reduced, the compactness and impermeability of the concrete can be improved, and the compressive strength and durability of the concrete can be enhanced, ensuring the long-term stability and safety of the engineering structure. Therefore, adjusting the water-cement ratio can not only optimize the physical properties of concrete, but also improve the efficiency and quality control of the construction process. Accurate water-cement ratio adjustment can reduce concrete waste and loss, reduce construction costs, and ensure the consistency and controllability of concrete to meet design requirements and engineering standards. DETAILED DESCRIPTION
[0056] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0057] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0058] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0059] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.
[0060] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.
[0061] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0062] Example 1
[0063] A low-carbon concrete, prepared from the following raw materials in parts by weight:
[0064] Cement: 100 parts,
[0065] Fly ash: 15 parts,
[0066] Modified recycled concrete aggregate: 15 parts,
[0067] Coarse sand: 10 parts,
[0068] Self-healing materials: 5 pieces.
[0069] The cement is PI42.5 type silicate cement.
[0070] The self-healing material is hollow polypropylene fiber with an aspect ratio of 15:1.
[0071] The particle size of coarse sand is 0.5mm to 2.5mm.
[0072] Wherein, the preparation method of modified recycled concrete aggregate is:
[0073] (1) soaking rubber powder in 10% sodium hydroxide solution to obtain pretreated high-performance rubber powder;
[0074] (2) mixing the regenerated micropowder and the alkaline activator uniformly and then grinding them to obtain alkali-activated regenerated micropowder, wherein the alkaline activator is a mixture of magnesium hydroxide and trimethylamine in a mass ratio of 1:1;
[0075] (3) adding a silane coupling agent to the alkali-activated regenerated micropowder, stirring evenly, then adding polyvinyl alcohol, and continuing to stir to obtain the pretreated regenerated micropowder;
[0076] (4) Natural sand and gravel, pre-treated recycled micro powder and slag powder are mixed evenly to obtain modified recycled concrete aggregate.
[0077] In step (1), the concentration of the sodium hydroxide solution is 10% to 20%. The rubber powder is waste rubber powder.
[0078] In step (2), the mass ratio of the regenerated micro powder to the alkaline activator is 50:5 to 10. The regenerated micro powder is obtained by crushing and screening waste concrete, and the particle size is less than 0.2 mm.
[0079] The preparation method of low-carbon concrete is: adding cement, fly ash, modified recycled concrete aggregate and coarse sand into a mixing tank for stirring, and after mixing, adding self-healing material until the self-healing material is evenly dispersed in the concrete slurry.
[0080] Example 2
[0081] A low-carbon concrete, which is different from Example 1 in that the raw materials for preparation are:
[0082] Cement: 100 parts,
[0083] Fly ash: 20 parts,
[0084] Modified recycled concrete aggregate: 20 parts,
[0085] Coarse sand: 15 parts,
[0086] Self-healing materials: 5 pieces.
[0087] Example 3
[0088] A low-carbon concrete, which is different from Example 1 in that the raw materials for preparation are:
[0089] Cement: 100 parts,
[0090] Fly ash: 25 parts,
[0091] Modified recycled concrete aggregate: 25 parts,
[0092] Coarse sand: 20 parts,
[0093] Self-healing materials: 10 pieces.
[0094] Comparative Example 1
[0095] A low-carbon concrete, which is different from Example 1 in that no modified recycled concrete aggregate is added to the raw materials.
[0096] Comparative Example 2
[0097] A low-carbon concrete, which is different from Example 1 in that the self-healing material is solid polypropylene fiber with the same aspect ratio.
[0098] Performance Testing
[0099] The flexural strength and compressive strength of the concrete of the embodiment and the comparative example were tested according to GB / T50082-2009 and GB / T50081-2019. The results are shown in Table 1 and Table 2.
[0100] Table 1
[0101] 3d flexural strength / MPa 7d flexural strength / MPa 21d flexural strength / MPa Example 1 5.88 7.68 10.04 Example 2 6.03 8.25 10.99 Example 3 6.24 8.37 11.24 Comparative Example 1 4.34 6.15 8.44 Comparative Example 2 4.61 6.78 8.81
[0102] Table 2
[0103]
[0104]
[0105] According to Tables 1 and 2, the amount of cement and fly ash in Example 3 is large, the modified recycled concrete aggregate and coarse sand are also large, and the proportion of self-healing materials is high, so the flexural strength and compressive strength are high. Example 2 has a large amount of cement and fly ash, moderate aggregate and coarse sand, a slightly lower proportion of self-healing materials, and slightly lower flexural strength and compressive strength than Example 3. Example 1 has a fixed amount of cement, a moderate proportion of fly ash and modified recycled concrete aggregate, less self-healing materials, and relatively low flexural strength and compressive strength. Comparative Example 1 does not use modified recycled concrete aggregate, so the flexural strength and compressive strength are lower than Example 1. The self-healing material of Comparative Example 2 is solid polypropylene fiber, and compared with hollow polypropylene fiber, the self-healing effect is poor, and the flexural strength and compressive strength are between Example 1 and Example 2.
[0106] The low-carbon concrete of the present invention is a new material with the main goal of reducing carbon emissions. It significantly reduces carbon emissions by reducing the amount of cement used and using alternative materials such as fly ash. Carbon dioxide emissions during cement production are one of the main sources of greenhouse gases, and alternative materials such as fly ash can not only reduce dependence on natural resources, but also effectively reduce the carbon footprint of concrete production.
[0107] Furthermore, the low-carbon concrete of the present invention can improve its interface performance and bonding strength with the cement matrix after the recycled concrete aggregate is modified, which not only effectively utilizes the waste concrete resources, but also improves the mechanical properties and durability of the concrete and prolongs the service life of the structure.
[0108] The addition of coarse sand in the formula can improve the working performance and compressive strength of concrete, while ensuring the fluidity and density of concrete.
[0109] Furthermore, the self-healing materials added to low-carbon concrete can fill and repair cracks after micro-cracks in the concrete occur, thereby delaying and preventing the expansion of cracks and improving the durability and maintenance cost of concrete.
[0110] Since low-carbon concrete uses environmentally friendly raw materials and technologies in its preparation process, it reduces the consumption of natural resources and the impact on the environment. At the same time, since it improves the durability of concrete and reduces maintenance requirements, it can reduce the overall carbon footprint and life cycle costs, which is in line with the concept of sustainable development.
[0111] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A low-carbon concrete, It is characterized in that The preparation raw materials include cement, fly ash, modified recycled concrete aggregate, coarse sand and self-healing materials.
2. The low carbon concrete according to claim 1, It is characterized in that In parts by weight, the raw materials for preparation include: 100 parts of cement, Fly ash: 10 to 30 parts, Modified recycled concrete aggregate: 10 to 30 parts, Coarse sand: 10 to 20 parts, Self-healing material: 5 to 10 parts.
3. The low carbon concrete according to claim 1 or 2, It is characterized in that The preparation method of the modified recycled concrete aggregate is: (1) soaking rubber powder in sodium hydroxide solution to obtain pretreated high-performance rubber powder; (2) mixing the regenerated micropowder and the alkaline activator uniformly and then grinding them to obtain alkali-activated regenerated micropowder, wherein the alkaline activator is a mixture of magnesium hydroxide and trimethylamine in a mass ratio of 1 to 3:1; (3) adding a silane coupling agent to the alkali-activated regenerated micropowder, stirring evenly, then adding polyvinyl alcohol, and continuing to stir to obtain pretreated regenerated micropowder; (4) Mixing natural sand and gravel, the pretreated recycled fine powder and slag powder evenly to obtain the modified recycled concrete aggregate.
4. The low carbon concrete according to claim 3, It is characterized in that In step (1), the concentration of the sodium hydroxide solution is 10% to 20%.
5. The low carbon concrete according to claim 3, It is characterized in that In step (2), the mass ratio of the regenerated micropowder to the alkaline activator is 50:5-10.
6. The low carbon concrete according to claim 1 or 2, It is characterized in that The self-healing material is hollow polypropylene fiber.
7. The low carbon concrete according to claim 6, It is characterized in that The aspect ratio of the hollow polypropylene fiber is 10 to 20:
1.
8. The low carbon concrete according to claim 1 or 2, It is characterized in that The particle size of the coarse sand is 0.5 mm to 2.5 mm.
9. A method for preparing the low carbon concrete according to any one of claims 1 to 8, It is characterized in that The method comprises: adding the cement, fly ash, modified recycled concrete aggregate and coarse sand into a mixing tank for stirring, and after mixing, adding the self-healing material until the self-healing material is evenly dispersed in the concrete slurry.
10. The method according to claim 9, It is characterized in that The method also includes adjusting the water-cement ratio according to construction requirements after adding the self-healing material.
Citation Information
Patent Citations
Heat-resistant and high-strength concrete having gradient enclosing structure, and preparation method thereof
CN106116333A
Building underground structure high-ductility self-repairing concrete
CN110550912A
Low-carbon concrete and preparation method thereof
CN115417642A
Ultrahigh-aperture-ratio lightweight pervious concrete as well as preparation method, special ingredient and application thereof