Low-shrinkage cement-based grouting material based on water purification sludge and preparation method of low-shrinkage cement-based grouting material

By adding the defrosting agent of sodium tripolyphosphate and sodium citrate and the coagulant of anhydrous sodium sulfate to the water purification sludge, the cellular structure is opened and the hydration reaction is accelerated, and the energy consumption and the energy consumption in the water purification sludge treatment are solved. Due to the complex process, cement-based grouting materials with high fluid state and good coagulation performance were prepared, achieving economical, efficient and environmentally friendly resource utilization.

CN118878285AActive Publication Date: 2024-11-01XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY

Patent Information

Application Number
CN202411138216.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-01
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing water purification sludge treatment technology has shortcomings in raw materials and applications, energy consumption and cost issues, technical feasibility and stability, and environmentally friendly, making it difficult to achieve economical, efficient and environmentally friendly resource utilization solutions.

Method used

Using low-shrinkage cement-based grouting material based on water purification sludge, the cellular structure of the water purification sludge is opened by adding a defrosting agent of sodium tripolyphosphate and sodium citrate, free water is mixed with cement, and combined with accelerator to accelerate By hydration reaction, a backfill grouting material with high fluid state and good coagulation properties was prepared.

Benefits of technology

It has achieved improved flow and dispersion uniformity of water purification sludge in less water, reduced energy consumption and cost, simplified the preparation process, and has a wide range of materials, non-toxic effects, and has broad practicality and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878285A_ABST
    Figure CN118878285A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of water purification sludge treatment, and discloses a low-shrinkage cement-based grouting material based on water purification sludge and a preparation method thereof.The grouting material is prepared from, by mass, 67 parts of water purification sludge, 13-16 parts of Portland cement, 16 parts of quartz sand, 0.02-0.04 part of flocculant breaking agent, 0.1-0.3 part of coagulant and 0.2-0.5 part of water reducing agent; each part of the flocculant breaking agent contains 0.01 part of sodium tripolyphosphate and 0.03 part of sodium citrate. The preparation method comprises the following steps: uniformly mixing the water purification sludge with the flocculant breaking agent; then adding Portland cement and quartz sand, and uniformly mixing to obtain mixed slurry; and adding a water reducing agent and a coagulant into the mixed slurry, and uniformly mixing to obtain the low-shrinkage cement-based grouting material based on the water purification sludge. A cellular structure in the PCA water purification sludge can be opened to release free water to be mixed with cement to obtain the backfill grouting material with high flow state and good coagulation performance, and the backfill grouting material is simple in preparation method, wide in material source, low in cost, free of toxic and harmful effects and wide in practicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water purification sludge treatment, and in particular relates to a low-shrinkage cement-based grouting material based on water purification sludge and a preparation method thereof. Background Art

[0002] While using key technologies such as coagulation, sedimentation, filtration and disinfection to produce purified water that meets the quality standards for drinking water, urban water treatment plants are faced with the problem of how to deal with the sludge generated during the water purification process. Water purification sludge, a harmless, high-water-content, brown-yellow mobile soil formed through coagulation and sedimentation, has a crystal structure similar to clay and is mainly composed of minerals such as SiO2 and Al2O3.

[0003] If the water treatment sludge is not properly treated and directly landfilled, it will not only cause serious environmental pollution, but also waste a lot of precious water and land resources. In addition, due to its poor compression performance and high water content, the disposal cost of water treatment sludge is further increased.

[0004] At present, the disposal methods of water treatment sludge mainly include landfill, land utilization and construction material utilization, but these methods require complex processes and additional energy consumption. However, if water treatment sludge can be directly applied, it can not only reduce the treatment cost, but also achieve effective utilization of resources. Therefore, it is of great significance to explore the resource utilization methods of water treatment sludge.

[0005] Chinese invention patent application CN115477382A provides a method for resource utilization of iron-rich sludge in water treatment plants. The invention discloses a method for resource utilization of iron-rich sludge in water treatment plants, which uses iron-rich sludge in water treatment plants to make it into granular or brick-shaped shapes; the sludge particles are prepared by sludge drying technology, and the finished product is granular ceramsite, which is used as artificial wetland filler, avoiding secondary pollution caused by general treatment methods of sludge in water intake plants, strengthening the denitrification and phosphorus removal of artificial wetlands and realizing low-cost phosphorus resource recovery at the same time, thereby realizing the mineralization of iron-rich sludge in water treatment plants.

[0006] Chinese invention patent application CN101423321 proposes a method for recycling sludge from a water purification pool. The invention is related to a method for recycling sludge from a water purification pool in a water plant, which mainly precipitates sludge from a water purification pool in a water plant into slurry, removes sand and gravel impurities through filtration, enters a reflux stirring slurry tank for stirring, and is sent to a high-temperature sterilization granulation tower through a high-pressure pump. After being sterilized and dried by hot air to form granular sludge, it is calcined to stabilize free aluminum ions and other substances in the granular sludge into stable and pollution-free artificial sand for resource recycling.

[0007] Chinese invention patent application CN106518150B proposes a composite ceramsite prepared from water purification sludge and diatomaceous earth. The present invention relates to a composite ceramsite prepared from water purification sludge and diatomaceous earth and a method thereof, belonging to the field of inorganic non-metallic materials. The preparation steps of the composite ceramsite include mixing, balling, drying, preheating, and roasting. The invention uses the water purification sludge generated in the production process of the water supply plant and the waste diatomaceous earth generated by the brewery for filtration as raw materials, which can effectively solve the treatment and disposal problems of these two solid wastes.

[0008] Chinese invention patent application CN114057416A proposes a method for preparing silicate cement clinker by using sludge incineration ash. The invention relates to the field of cement technology, and specifically to a method for preparing silicate cement clinker by using sludge incineration ash. The present invention uses sludge incineration ash produced by urban sewage treatment as iron correction material to prepare cement clinker, and on the other hand, provides technical support for using cement kilns to coordinately treat urban wastewater sludge incineration ash, promote urban sludge reduction and sludge incineration ash resource utilization.

[0009] Chinese invention patent application CN106946434A proposes a method for resource utilization of manganese, aluminum and iron sludge in a water treatment plant. The invention discloses a method for resource utilization of manganese, aluminum and iron sludge in a water treatment plant, the steps of which include: using manganese, aluminum and iron sludge in a water treatment plant as raw material, first dehydrating to obtain dry sludge, then adding fly ash from a power plant and sulfuric acid in turn for acidification treatment to obtain acidified material, then adding kaolin, using sodium silicate to adjust the silicon: aluminum mass ratio in the silicified material to 1:1, standing for reaction for 7 days, drying or baking to obtain dry material, finally heating the dry material to 400-500℃ and calcining for 1h, and naturally cooling to obtain a material with adsorption capacity.

[0010] The shortcomings of the above patent applications are mainly concentrated in the following aspects:

[0011] Table 1

[0012]

[0013] In summary, the shortcomings of the above patent applications are mainly concentrated in the limitations of raw materials and applications, energy consumption and cost issues, technical feasibility and stability, and environmental friendliness. In practical applications, these factors need to be comprehensively considered to seek more economical, efficient and environmentally friendly sludge treatment and resource utilization solutions. Summary of the invention

[0014] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a low-shrinkage cement-based grouting material based on water purification sludge and a preparation method thereof. The present invention can open the cellular structure in PCA water purification sludge to release free water and mix it with cement to obtain a backfill grouting material with high fluidity and good coagulation performance. The present invention does not have the energy consumption problems of the above-mentioned prior art. In addition, the preparation method of the present invention is simple, the required materials are from a wide source, the cost is low, and there is no toxic effect, and it has wide practicality.

[0015] The technical solution adopted by the present invention is as follows:

[0016] A low shrinkage cement-based grouting material based on water purification sludge, the raw materials of which include, by weight:

[0017] 67 parts of water purification sludge, 13-16 parts of Portland cement, 16 parts of quartz sand, 0.02-0.04 parts of flocculant, 0.1-0.4 parts of coagulant, 0.2-0.5 parts of water reducing agent;

[0018] The flocculant comprises sodium tripolyphosphate and sodium citrate, and each portion of the flocculant contains 0.01 to 0.03 portions of sodium tripolyphosphate and 0.01 to 0.03 portions of sodium citrate.

[0019] Preferably, in terms of mass percentage, the water purification sludge contains minerals such as SiO2 and Al2O3 that are similar to the composition of clay. Specifically, the solid component of the water purification sludge contains 87% to 94% SiO2, 6% to 12% Al2O3, and the remainder is other impurities. The main elements of the water purification sludge are Si, Al, Fe, O, and C. The water content of the water purification sludge can reach up to 260%.

[0020] Preferably, the silicate cement is P·O 42.5R cement.

[0021] Preferably, the quartz sand is ISO standard sand.

[0022] Preferably, the water reducer is a naphthalene-based water reducer.

[0023] Preferably, the sodium tripolyphosphate is of industrial grade above 99%.

[0024] The sodium citrate is of industrial grade above 99%.

[0025] Preferably, the coagulant is anhydrous sodium sulfate.

[0026] Preferably, the coagulant is 99% or more industrial grade anhydrous sodium sulfate.

[0027] The method for preparing the low shrinkage cement-based grouting material based on water purification sludge of the present invention comprises the following steps:

[0028] The water purification sludge is mixed with a flocculant; then silicate cement and quartz sand are added and mixed to obtain a mixed slurry; then a water reducing agent and a coagulant are added to the mixed slurry, and the low shrinkage cement-based grouting material based on the water purification sludge is obtained by mixing.

[0029] The present invention has the following beneficial effects:

[0030] The present invention is based on the low shrinkage cement-based grouting material of water purification sludge, and a flocculant is added to the flocculant, which includes sodium tripolyphosphate and sodium citrate, wherein the addition of sodium tripolyphosphate causes the sodium tripolyphosphate to be hydrolyzed into phosphate ions and sodium ions, and the sodium ions generated by the hydrolysis replace the aluminum ions in the water purification sludge, and the aluminum ions are chelated with the phosphate to form a compatible complex, thereby destroying the cellular structure of the flocculated water purification sludge, supplementing the steric hindrance effect, and making the water purification sludge have higher fluidity in less water and be evenly dispersed. The phosphate ions generated after the hydrolysis of sodium tripolyphosphate replace the aluminum ions coagulated and flocculated after the hydrolysis of PAC (polyaluminum chloride) in the water purification sludge to form new soluble substances, destroying the original aluminum hydroxide colloidal structure generated by the hydrolysis of aluminum ions, releasing the enclosed free water, and then adding cement, and the cement plays a role in coagulating and solidifying the sludge. However, under the influence of high sludge moisture content, residual flocculant and sodium tripolyphosphate on the slow setting effect of cement, the cement setting and hardening time is seriously weakened, and it can only be formed in 7 days, but still cannot coagulate. Therefore, a coagulant is added in the present invention, and the coagulant can react with cement hydration to generate Ca(OH)2 to generate gypsum and alkali faster. The newly generated fine-grained dihydrate gypsum reacts much faster to cement than the gypsum added during cement grinding, and the hydration reaction generates hydrated calcium sulfoaluminate crystals. At the same time, the occurrence of the above reaction can also accelerate the hydration of C3S. Accelerating the hydration process improves the early strength without affecting its flow properties. The initial fluidity of the mixed slurry should be greater than 290mm, and the loss over 30min should be not less than 260mm, etc. The basic process requirements of grouting materials, 28d strength is above 1.5MPa.

[0031] In the preparation method of the present invention, the prepared deflocculant is firstly put into the flocculated sludge and stirred to destroy the cellular structure and release free water, and then cement and admixture are added to further stir and mix thoroughly.

[0032] In summary, the present invention can open the cellular structure in PCA water purification sludge to release free water and mix it with cement to obtain a backfill grouting material with high fluidity and good coagulation performance. The present invention does not have the energy consumption problems of the prior art pointed out in the above background technology. In addition, the preparation method of the present invention is simple, the required materials are from a wide range of sources, the cost is low, and there is no toxic effect, and it has wide practicality. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1The present invention is a flow chart of a method for preparing a low shrinkage cement-based grouting material based on water purification sludge. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is described below in conjunction with specific implementation examples. Each embodiment is an experimental example and provides real performance test data. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0035] The low shrinkage cement-based grouting material based on water purification sludge of the present invention comprises the following raw materials in proportion by weight: 67 parts of water purification sludge, 13-16 parts of Portland cement, 16 parts of quartz sand, 0.02-0.04 parts of flocculants, 0.1-0.4 parts of coagulants, and 0.2-0.5 parts of water reducers, wherein the flocculants comprise sodium tripolyphosphate and sodium citrate, and each part of the flocculants contains 0.01-0.03 parts of sodium tripolyphosphate and 0.01-0.03 parts of sodium citrate.

[0036] The silicate cement is P·O 42.5R cement, the quartz sand is ISO standard sand, the water reducer is naphthalene-based water reducer, the sodium tripolyphosphate is 99% or more industrial grade, the sodium citrate is 99% or more industrial grade, and the coagulant is 99% or more industrial grade anhydrous sodium sulfate.

[0037] Reference Figure 1 The method for preparing the low shrinkage cement-based grouting material based on water purification sludge of the present invention comprises the following steps:

[0038] Weigh ordinary Portland cement, purified water flocculation sludge, flocculant, quartz sand, water reducing agent and coagulant according to the proportion;

[0039] Put the water purification sludge into NJ-160A mixer, then pour the flocculant into NJ-160A mixer and mix, stir at a low speed of 65r / min for 240 seconds until it is uniform, and obtain high-fluidity flocculant sludge;

[0040] Then add ordinary Portland cement and quartz sand into NJ-160A mixer, stir at a low speed of 65r / min for 120 seconds until the mixture is uniform, and obtain a mixed slurry;

[0041] Then, the water reducing agent and the coagulant are poured into the NJ-160A mixer, and the cement slurry mixer is stirred at a high speed of 130 r / min for 120 seconds until the mixture is uniform, thereby obtaining the low shrinkage cement-based grouting material based on water purification sludge of the present invention.

[0042] The specific mechanism of the technical solution of the present invention is explained as follows:

[0043] The technical problem to be solved by the present invention is to open the cellular structure in PCA water purification sludge to release free water and mix it with cement to obtain a backfill grouting material with high fluidity and good coagulation performance. A flocculant prepared by sodium tripolyphosphate and sodium citrate in a certain proportion is added to the water purification sludge. The addition of sodium tripolyphosphate allows the phosphate radicals hydrolyzed by sodium tripolyphosphate to replace the aluminum ions in the water purification sludge through ion exchange, and the aluminum ions are chelated with the phosphate radicals to form a compatible complex, which destroys the flocculated cellular structure in the water purification sludge and supplements the steric hindrance effect. The water purification sludge has a higher fluidity in less water and is evenly dispersed. The phosphate ions generated after the hydrolysis of sodium tripolyphosphate replace the aluminum ions coagulated and flocculated after the hydrolysis of PAC (polyaluminum chloride) in the water purification sludge to form new soluble substances, destroying the original aluminum hydroxide colloidal structure generated by the hydrolysis of aluminum ions, releasing the enclosed free water, and then adding silicate cement, which plays a role in coagulating and solidifying the sludge. However, under the influence of high sludge moisture content, residual flocculant and sodium tripolyphosphate on the slow setting effect of cement, the setting and hardening time of cement is seriously weakened. It can only be formed in 7 days, but still cannot coagulate. Therefore, the present invention also adds an accelerating component-anhydrous sodium sulfate. Sodium sulfate reacts with cement to generate Ca(OH)2 quickly to generate gypsum and alkali. The newly generated fine-grained dihydrate gypsum reacts much faster to cement than the gypsum added during cement grinding. The hydration reaction generates hydrated calcium sulfoaluminate crystals. At the same time, the occurrence of the above reaction can also accelerate the hydration of C3S. Accelerating the hydration process improves the early strength without affecting its flow properties. The initial fluidity of the mixed slurry should be greater than 290mm, and the loss over 30min should be no less than 260mm, etc. The basic process requirements of grouting materials, 28d strength is above 1.5MPa.

[0044] It can be seen from the above mechanism that, compared with the prior art, the present invention solves the problems of additional energy input and complex processes in the resource utilization of water purification sludge compared with the previous resource utilization of water purification sludge.

[0045] The following is further explained in conjunction with specific embodiments. The water purification sludge used in the following embodiments of the present invention is water purification sludge produced by a tap water treatment plant. Calculated by mass percentage, the solid component of the water purification sludge contains: 93% SiO2, 6.5% Al2O3, and the remainder is other impurities; the water content of the water purification sludge is 260%.

[0046] Embodiment 1:

[0047] The low shrinkage cement-based grouting material based on water purification sludge in this embodiment includes, by weight, 67 parts of water purification sludge, 13 parts of Portland cement, 16 parts of quartz sand, 0.02 parts of flocculants, 0.1 parts of anhydrous sodium sulfate, and 0.2 parts of naphthalene-based water reducer. Each part of flocculants contains 0.01 parts of sodium tripolyphosphate and 0.03 parts of sodium citrate.

[0048] The low shrinkage cement-based grouting material based on water purification sludge in this embodiment is prepared according to the above-mentioned preparation method.

[0049] Embodiment 2:

[0050] The low shrinkage cement-based grouting material based on water purification sludge in this embodiment includes, by weight, 67 parts of water purification sludge, 14 parts of Portland cement, 16 parts of quartz sand, 0.03 parts of flocculants, 0.2 parts of anhydrous sodium sulfate, and 0.3 parts of naphthalene-based water reducer. Each part of flocculants contains 0.02 parts of sodium tripolyphosphate and 0.02 parts of sodium citrate.

[0051] The low shrinkage cement-based grouting material based on water purification sludge in this embodiment is prepared according to the above-mentioned preparation method.

[0052] Embodiment 3:

[0053] The low shrinkage cement-based grouting material based on water purification sludge in this embodiment includes, by weight, 67 parts of water purification sludge, 15 parts of Portland cement, 16 parts of quartz sand, 0.04 parts of flocculants, 0.3 parts of anhydrous sodium sulfate, and 0.4 parts of naphthalene-based water reducer. Each part of flocculants contains 0.03 parts of sodium tripolyphosphate and 0.01 parts of sodium citrate.

[0054] The low shrinkage cement-based grouting material based on water purification sludge in this embodiment is prepared according to the above-mentioned preparation method.

[0055] Embodiment 4:

[0056] The low shrinkage cement-based grouting material based on water purification sludge in this embodiment includes, by weight, 67 parts of water purification sludge, 16 parts of Portland cement, 16 parts of quartz sand, 0.02 parts of flocculants, 0.4 parts of anhydrous sodium sulfate, and 0.5 parts of naphthalene-based water reducer. Each part of flocculants contains 0.015 parts of sodium tripolyphosphate and 0.035 parts of sodium citrate.

[0057] The low shrinkage cement-based grouting material based on water purification sludge in this embodiment is prepared according to the above-mentioned preparation method.

[0058] The performance test of the low shrinkage cement-based grouting material based on clean water sludge prepared in the above Examples 1 to 4 shows that the fluidity meets the requirements of the current national standard "Method for Determining Fluidity of Cement Mortar" GB / T2419, the initial fluidity ranges from 330 to 290 mm, the fluidity ranges from 260 to 290 mm after 30 min, the density and shrinkage at 28 days are in accordance with the "Test Method for Drying Shrinkage and Cracking Performance of Cement Mortar and Concrete" GB / T 29417-2012, and the compressive strength test shall be carried out in accordance with the relevant provisions of the current national standard "Test Method for Strength of Cement Mortar (ISO Method)" GB / T17671, ranging from 0.5 to 2.5 MPa. The specific test results are shown in Table 2:

[0059] Table 2

[0060]

[0061]

[0062] It can be seen from the test results in Table 1 that in each embodiment, as the cement ratio increases, the water-cement ratio of the slurry decreases relatively, and the fluidity decreases accordingly. The initial fluidity ranges from 310 to 290 mm, and the time loss ranges from 260 to 290 mm; the density increases accordingly with the increase of solid content, ranging from 0.83 to 0.90 / kg·m -3 ; As the proportion of cement increases, the amount of hydration products produced increases, and the compressive strength increases accordingly. The strength range is 0.9 to 1.8 MPa, which meets the fluidity and strength standards of grouting materials.

[0063] The shrinkage test results of the materials prepared in the above-mentioned Examples 1 to 4 are shown in Table 3:

[0064] Table 3

[0065]

[0066] It can be seen from the data in Table 2 that as the cement content increases, the solid content of the slurry also increases accordingly, and the shrinkage rate also decreases accordingly, ranging from 2.55% to 3.85%, which meets the shrinkage standard of cement grouting materials.

Claims

1. A low shrinkage cement-based grouting material based on water purification sludge, characterized in that: The raw materials include, by weight: 67 parts of water purification sludge, 13-16 parts of Portland cement, 16 parts of quartz sand, 0.02-0.04 parts of flocculant, 0.1-0.4 parts of coagulant, 0.2-0.5 parts of water reducing agent; The flocculant comprises sodium tripolyphosphate and sodium citrate, and each portion of the flocculant contains 0.01 to 0.03 portions of sodium tripolyphosphate and 0.01 to 0.03 portions of sodium citrate.

2. A low shrinkage cement-based grouting material based on water purification sludge according to claim 1, characterized in that: In terms of mass percentage, the solid components of the water purification sludge contain: 87% to 94% SiO2, 6% to 12% Al2O3, and the remainder is other impurities. The water content of the water purification sludge can reach up to 260%.

3. A low shrinkage cement-based grouting material based on water purification sludge according to claim 1, characterized in that: The silicate cement is P·O 42.5R cement.

4. A low shrinkage cement-based grouting material based on water purification sludge according to claim 1, characterized in that: The quartz sand adopts ISO standard sand.

5. The low shrinkage cement-based grouting material based on water purification sludge according to claim 1, characterized in that: The water reducing agent is a naphthalene-based water reducing agent.

6. A low shrinkage cement-based grouting material based on water purification sludge according to claim 1, characterized in that: The sodium tripolyphosphate is of industrial grade above 99%.

7. A low shrinkage cement-based grouting material based on water purification sludge according to claim 6, characterized in that: The sodium citrate is of industrial grade above 99%.

8. A low shrinkage cement-based grouting material based on water purification sludge according to claim 6 or 7, characterized in that: The coagulant is anhydrous sodium sulfate.

9. The low shrinkage cement-based grouting material based on water purification sludge according to claim 1, characterized in that: The coagulant is an industrial grade anhydrous sodium sulfate of more than 99%.

10. The method for preparing a low shrinkage cement-based grouting material based on water purification sludge according to any one of claims 1 to 9, characterized in that: The process includes the following: The water purification sludge is mixed with a flocculant; then silicate cement and quartz sand are added and mixed to obtain a mixed slurry; then a water reducing agent and a coagulant are added to the mixed slurry, and the low shrinkage cement-based grouting material based on the water purification sludge is obtained by mixing.

Citation Information

Patent Citations

  • Mortar retarder

    CN103265203A

  • Integral treatment method of dehydration and solidification of sludge

    CN104944736A

  • Concrete repairing material suitable for ocean environment and preparation method thereof

    CN107572992A

  • Treatment process for reusing sludge as resources

    CN109879579A

  • Low-temperature sleeve grouting material and preparation method

    CN111807794A

Cited By

  • Preparation method and application of self-leveling filling waste pipeline material

    CN120117855A