Wear-resistant casting molding brick for cement kiln and manufacturing method thereof
By using wear-resistant cast molded bricks for cement kilns, the problem of the decline in strength of traditional cement kiln head materials at high temperatures is solved, and the wear resistance performance and production efficiency are improved. The raw materials are easy to obtain, the cost is low, and the process is simple.
Patent Information
- Application Number
- CN202411055182.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The strength of traditional cement kiln head materials decreases after washing high-temperature cement clinker, short service life, resulting in low production efficiency and requires frequent maintenance and replacement.
Wear-resistant cast molded bricks are used for cement kilns. The raw materials include white corundum powder, alumina powder, high-alumina cement and stainless steel fibers. They are made through specific stirring and drying processes to increase wear resistance.
It significantly improves wear resistance and service life, improves production efficiency, and is simple and easy to obtain raw materials, low production costs, and simple and easy to perform process steps.
Smart Images

Figure CN118878291A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cement kiln production equipment, in particular to wear-resistant cast-molded bricks for cement kilns and a manufacturing method thereof. Background Art
[0002] Cement rotary kiln is an important equipment for firing cement clinker. Cement clinker enters the rotary kiln from the kiln head end. The temperature of cement clinker is about 1000-1100℃. The refractory material at the kiln head feed port needs to resist the erosion of high-temperature cement clinker. At present, many manufacturers choose low-cement castables to make kiln head feed ports. After a period of use, the traditional kiln head materials are washed by high-temperature cement clinker, and the strength decreases. The service life is short and it is not wear-resistant. It always needs to be repaired and replaced, resulting in low production efficiency.
[0003] Therefore, wear-resistant cast bricks for cement kilns are proposed to solve the above problems. Summary of the invention
[0004] The purpose of the present invention is to provide wear-resistant cast bricks for cement kilns and a method for making the same, so as to solve the problem in the above-mentioned background technology that after a period of use, the traditional kiln head materials are washed by high-temperature cement clinker, their strength decreases, their service life is short, they are not wear-resistant, and they always need to be repaired and replaced, resulting in low production efficiency.
[0005] To achieve the above object, the present invention provides the following technical solutions: 1. Wear-resistant cast bricks for cement kilns and a method for making the same, characterized in that:
[0006] A: Raw materials for wear-resistant cast bricks for cement kilns: including the following percentages: 20-30% white corundum powder, 20-30% alumina powder, 40-60% high alumina cement, 1-3% additives;
[0007] B: The production method of wear-resistant cast bricks for cement kiln is:
[0008] S1: Mixture preparation: weigh and premix appropriate amounts of white corundum powder, alumina powder, high alumina cement and additives;
[0009] S2: Prepare the forming mold, spray the release agent on the inner wall of the mold, and then fill an appropriate amount of stainless steel fiber into the forming mold, with the filling height being 0.5 cm from the top of the forming mold;
[0010] S3: Put the prepared mixture into the mixer, first use slow gear to stir, the slow gear pre-stirring time is one minute, add 80% of the total required water, and use fast gear to stir after adding water inside the mixer, the fast gear stirring time is two minutes, and then add the remaining 20% of water after stirring, continue to use fast gear to stir for one minute, and discharge after successful stirring;
[0011] S4: discharging the kneaded product after adding water and stirring into a mold, and filling the mold to a full state;
[0012] S5: Let the filled mold stand for 24 hours, then put it into a drying oven and set it to 50℃ / 24h for drying.
[0013] S6: Take out the mold, remove the mold, put the finished product into the grinding area, use a grinder to grind the surface to be flush with the upper part of the mold, and repair the products with pores and exposed iron wires; lay the products flat on the iron tray, use high-temperature asbestos strips in the middle, and dry them at 300℃ / 24h in the later stage.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] 1) The raw materials are easy to obtain, the production cost is not high, the requirements for the production environment are low, the production steps are not complicated, and it is simple and easy to use.
[0016] 2) Compared with existing cement kiln bricks, the wear resistance and strength are greatly improved after adding steel fiber, the service life is longer, and the work efficiency can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic diagram of the production process of the present invention;
[0018] Figure 2 It is a schematic diagram of the strength comparison structure of the present invention;
[0019] Figure 3 It is a schematic diagram of the cross-sectional structure of the present invention. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "top / bottom" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific position, be constructed and operated in a specific position, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0022] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "mounted / connected", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0023] Example:
[0024] See also Figure 1-3 The present invention provides a technical solution: 1. Wear-resistant cast bricks for cement kilns and a method for making the same, characterized in that:
[0025] A: Raw materials for wear-resistant cast bricks for cement kilns: including the following percentages: 20-30% white corundum powder, 20-30% alumina powder, 40-60% high alumina cement, 1-3% additives;
[0026] B: The production method of wear-resistant cast bricks for cement kiln is:
[0027] S1: Mixture preparation: weigh and premix appropriate amounts of white corundum powder, alumina powder, high alumina cement and additives. Accurate weighing is required before premixing to ensure that all raw materials are accurately weighed according to the formula. Dust will be generated during the premixing process, and appropriate dust removal measures should be taken. After premixing, the mixture needs to be quality tested to ensure that it meets the expected standards.
[0028] S2: Prepare the molding mold, spray the mold release agent on the inner wall of the mold, and then fill the molding mold with an appropriate amount of stainless steel fiber, with the filling height being 0.5 cm from the top of the molding mold; stainless steel fiber can effectively inhibit the development of micro cracks in the molding bricks, thereby improving the overall crack resistance of the molding bricks. During the hardening process of concrete, cracks are prone to occur due to shrinkage or external stress. Stainless steel fiber can effectively reduce the appearance of these cracks. The tensile strength of concrete itself is low. Adding stainless steel fiber can significantly improve the ability of the molding bricks to resist tensile damage. Stainless steel fiber can bridge the cracks in the molding bricks and prevent the cracks from further expanding, thereby improving the tensile strength. Adding stainless steel fiber can also improve the bending resistance of the molding bricks, making the molding bricks stronger when subjected to bending loads. Stainless steel fiber is randomly distributed in concrete, which can effectively disperse stress and reduce brittle fracture. Stainless steel fiber can improve the ability of the molding bricks to resist impact, making them less likely to break when subjected to external force impact. Adding stainless steel fiber can improve the toughness of the molding bricks, which means that even under the action of large external forces, the molding bricks are not prone to sudden brittle failure. Stainless steel fiber itself has good corrosion resistance, which enables the molding bricks containing stainless steel fiber to maintain good performance in harsh environments.
[0029] S3: Put the prepared mixture into the mixer, first use slow gear to stir, the slow gear pre-stirring time is one minute, add 80% of the total required water, and use fast gear to stir after adding water inside the mixer, the fast gear stirring time is two minutes, and then add the remaining 20% of water after stirring, continue to use fast gear to stir for one minute, and discharge after successful stirring;
[0030] S4: discharging the kneaded product after adding water and stirring into a mold, and filling the mold to a full state;
[0031] S5: Let the filled mold stand for 24 hours, then put it into a drying oven and set it to 50℃ / 24h for drying.
[0032] S6: Take out the mold, remove the mold, put the finished product into the grinding area, use a grinder to grind the surface to be flush with the upper part of the mold, and repair the products with pores and exposed iron wires; lay the products flat on the iron tray, use high-temperature asbestos strips in the middle, and dry them at 300℃ / 24h in the later stage.
[0033] Embodiment 1
[0034] A: Raw materials for wear-resistant cast bricks for cement kilns: including the following percentages: 25% white corundum powder, 25% alumina powder, 49% high alumina cement, and 1% additives;
[0035] B: The production method of wear-resistant cast bricks for cement kiln is:
[0036] S1: Mixture preparation: weigh and premix appropriate amounts of white corundum powder, alumina powder, high alumina cement and additives;
[0037] S2: Prepare the forming mold, spray the release agent on the inner wall of the mold, and then fill an appropriate amount of stainless steel fiber into the forming mold, with the filling height being 0.5 cm from the top of the forming mold;
[0038] S3: Put the prepared mixture into the mixer, first use slow gear to stir, the slow gear pre-stirring time is one minute, add 80% of the total required water, and use fast gear to stir after adding water inside the mixer, the fast gear stirring time is two minutes, and then add the remaining 20% of water after stirring, continue to use fast gear to stir for one minute, and discharge after successful stirring;
[0039] S4: discharging the kneaded product after adding water and stirring into a mold, and filling the mold to a full state;
[0040] S5: Let the filled mold stand for 24 hours, then put it into a drying oven and set it to 50℃ / 24h for drying.
[0041] S6: Take out the mold, remove the mold, put the finished product into the grinding area, use a grinder to grind the surface to be flush with the upper part of the mold, and repair the products with pores and exposed iron wires; lay the products flat on the iron tray, use high-temperature asbestos strips in the middle, and dry them at 300℃ / 24h in the later stage.
[0042] Embodiment 2
[0043] A: Raw materials for wear-resistant cast bricks for cement kilns: including the following percentages: white corundum powder 30%, alumina powder 28%, high alumina cement 40%, additives 2%;
[0044] B: The production method of wear-resistant cast bricks for cement kiln is:
[0045] S1: Mixture preparation: weigh and premix appropriate amounts of white corundum powder, alumina powder, high alumina cement and additives;
[0046] S2: Prepare the forming mold, spray the release agent on the inner wall of the mold, and then fill an appropriate amount of stainless steel fiber into the forming mold, with the filling height being 0.5 cm from the top of the forming mold;
[0047] S3: Put the prepared mixture into the mixer, first use slow gear to stir, the slow gear pre-stirring time is one minute, add 80% of the total required water, and use fast gear to stir after adding water inside the mixer, the fast gear stirring time is two minutes, and then add the remaining 20% of water after stirring, continue to use fast gear to stir for one minute, and discharge after successful stirring;
[0048] S4: discharging the mixed product after adding water and stirring into a mold, and filling the inside of the mold to a full state;
[0049] S5: Let the filled mold stand for 24 hours, then put it into a drying oven and set it to 50℃ / 24h for drying.
[0050] S6: Take out the mold, remove the mold, put the finished product into the grinding area, use a grinder to grind the surface to be flush with the upper part of the mold, and repair the products with pores and exposed iron wires; lay the products flat on the iron tray, use high-temperature asbestos strips in the middle, and dry them at 300℃ / 24h in the later stage.
[0051] Embodiment 3
[0052] A: Raw materials for wear-resistant cast bricks for cement kilns: including the following percentages: white corundum powder 29%, alumina powder 29%, high alumina cement 42%, additives 1%;
[0053] B: The production method of wear-resistant cast bricks for cement kiln is:
[0054] S1: Mixture preparation: weigh and premix appropriate amounts of white corundum powder, alumina powder, high alumina cement and additives;
[0055] S2: Prepare the forming mold, spray the release agent on the inner wall of the mold, and then fill an appropriate amount of stainless steel fiber into the forming mold, with the filling height being 0.5 cm from the top of the forming mold;
[0056] S3: Put the prepared mixture into the mixer, first use slow gear to stir, the slow gear pre-stirring time is one minute, add 80% of the total required water, and use fast gear to stir after adding water inside the mixer, the fast gear stirring time is two minutes, and then add the remaining 20% of water after stirring, continue to use fast gear to stir for one minute, and discharge after successful stirring;
[0057] S4: discharging the kneaded product after adding water and stirring into a mold, and filling the mold to a full state;
[0058] S5: Let the filled mold stand for 24 hours, then put it into a drying oven and set it to 50℃ / 24h for drying.
[0059] S6: Take out the mold, remove the mold, put the finished product into the grinding area, use a grinder to grind the surface to be flush with the upper part of the mold, and repair the products with pores and exposed iron wires; lay the products flat on the iron tray, use high-temperature asbestos strips in the middle, and dry them at 300℃ / 24h in the later stage.
[0060] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the attached claims rather than the above description. Therefore, it is intended to include all changes within the meaning and scope of the equivalent elements of the claims in the present invention, and any figure marks in the claims should not be regarded as limiting the claims involved.
[0061] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Wear-resistant cast bricks for cement kiln and production method thereof, characterized in that: A: Raw materials for wear-resistant cast bricks for cement kilns: including the following percentages: 20-30% white corundum powder, 20-30% alumina powder, 40-60% high alumina cement, 1-3% additives; B: The production method of wear-resistant cast bricks for cement kiln is: S1: Mixture preparation: weigh and premix appropriate amounts of white corundum powder, alumina powder, high alumina cement and additives; S2: Prepare the forming mold, spray the release agent on the inner wall of the mold, and then fill an appropriate amount of stainless steel fiber into the forming mold, with the filling height being 0.5 cm from the top of the forming mold; S3: Put the prepared mixture into the mixer, first use slow gear to stir, the slow gear pre-stirring time is one minute, add 80% of the total required water, and use fast gear to stir after adding water inside the mixer, the fast gear stirring time is two minutes, and then add the remaining 20% of water after stirring, continue to use fast gear to stir for one minute, and discharge after successful stirring; S4: discharging the kneaded product after adding water and stirring into a mold, and filling the mold to a full state; S5: Let the filled mold stand for 24 hours, then put it into a drying oven and set it to 50℃ / 24h for drying. S6: Take out the mold, remove the mold, put the finished product into the grinding area, use a grinder to grind the surface to be flush with the upper part of the mold, and repair the products with pores and exposed iron wires; lay the products flat on the iron tray, use high-temperature asbestos strips in the middle, and dry them at 300℃ / 24h in the later stage.
Citation Information
Patent Citations
High-strength wear-resistant pouring material for aerial refuse incinerator
CN101302112A
Unfired high-strength metal ceramic composite material as well as preparation method and application thereof