Preparation method of coal gasification slag-lithium slag-steel slag based lightweight concrete
The coordinated preparation of lightweight concrete by coal gasification slag, lithium slag, steel slag, etc. has solved the problem of industrial solid waste treatment, achieved resource utilization and environmental protection, and improved the performance and economic benefits of concrete.
Patent Information
- Application Number
- CN202410722543.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to effectively utilize and process a large amount of industrial solid waste such as cyanide tailings, lithium slag and steel slag, resulting in environmental pollution and waste of resources.
Coal gasification slag, lithium slag, steel slag, etc. are used to prepare lightweight concrete in a coordinated manner. Through pretreatment and high-temperature calcination, high-performance low-carbon powder is formed, replacing traditional silicate cement clinker, and realizing solid waste resource utilization .
It has achieved harmless, reduced and resource utilization of solid waste, reduced production costs, improved the mechanical properties and economic benefits of concrete, and complied with the safety and environmental protection standards of building materials.
Smart Images

Figure CN118878293A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of comprehensive resource utilization, and in particular relates to a method for preparing coal gasification slag-lithium slag-steel slag-based lightweight concrete. Background Art
[0002] Cyanide tailings are waste slag discharged after domestic gold smelting. The national gold industry discharges a large amount of cyanide slag every year. With the continuous development of production, the annual discharge of cyanide slag has increased. Especially in recent years, with the continuous improvement of production technology, cyanidation has been widely adopted, and the corresponding large-scale discharge of cyanide tailings has brought some serious problems. Whether it is the cyanide tailings of flotation gold concentrate or the full mud cyanide slag, their common feature is that the slag particle size is very fine. Cyanide slag is generally stored in the form of tailings pond as solid waste. The particle size of cyanide slag becomes finer and the surface area increases during the beneficiation process. It is easy to flow and collapse when stored in large quantities, causing vegetation damage and injury accidents. With the increase in the amount of cyanide slag, the dam height also increases accordingly. The valuable elements comprehensively recovered from cyanide slag include gold, silver, copper, lead, zinc, sulfur, and iron. However, the iron phase wraps the metal phase, resulting in a very low direct cyanide gold recovery rate.
[0003] my country's new energy vehicle industry is developing rapidly. Lithium ore is currently the main lithium raw material in my country. However, the extraction of lithium from lithium ore produces a large amount of lithium smelting slag (usually 8 to 10 tons of lithium slag will be produced for every ton of lithium salt produced). At present, the recycling and treatment of lithium slag is mainly landfill or open-air stacking. Only a small amount of lithium slag will be used as raw materials for concrete, cement and ceramics. The remaining lithium slag is difficult to be reasonably recycled. Its random stacking not only occupies a large amount of land resources, but also the sulfur element it contains will pollute the surrounding soil with soil erosion.
[0004] Steel slag is obtained by melting scrap with high electric current in an electric arc furnace or by treating hot molten metal, scrap and flux with lime in a basic oxygen furnace. About 70% of the world's steel production depends on the blast furnace process, as the availability of scrap limits electric arc furnace production to 30% of global demand. In the converter process, for every ton of steel produced, the amount of converter slag produced is between 0.1 and 0.2 tons.
[0005] Coal gasification ash is a by-product of the coal gasification process. my country emits huge amounts of ash every year. Most of the coal gasification ash is disposed of by landfilling or storing it in slag yards, but landfilling and storage can also cause serious environmental pollution and safety hazards.
[0006] Phosphogypsum is a slurry-like mixture produced by the reaction of phosphate rock and sulfuric acid during the production of phosphate fertilizer. It contains liquid phosphoric acid and solid calcium sulfate residue. After filtering and washing, H3PO4 and CaSO4 can be separated, and the resulting CaSO4 residue is phosphogypsum. Its main chemical composition is CaSO4·2H2O. It has a higher water content than natural gypsum, but phosphogypsum contains some impurities, which hinder its use. The impurities in phosphogypsum mainly include soluble impurities, insoluble impurities and eutectic phosphorus.
[0007] How to effectively utilize multiple solid wastes such as cyanide tailings, steel slag, coal gasification ash, phosphogypsum, etc., greatly reduce environmental pollution, turn waste into treasure, and achieve significant economic and social benefits, this technical problem urgently needs to be solved. Summary of the invention
[0008] The present invention utilizes cyanide tailings, alkali slag, calcium-silicon slag, lithium slag, coal gasification ash slag, phosphogypsum and the like to collaboratively prepare concrete, which can not only solve the problems of harmlessness, reduction and resource utilization of bulk industrial solid waste, but also promote the coordinated utilization of hazardous waste and industrial solid waste and environmental protection, provide raw materials for large-scale replacement of cement-based concrete, and lay the foundation for the project.
[0009] The present invention provides a method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete, the preparation method comprising the following steps:
[0010] S1. Cyanide tailings / steel slag pretreatment: First, the cyanide tailings and steel slag are dried to constant weight, crushed to particles ≤ 2 mm by a crusher, and then the cyanide tailings and steel slag are mixed at a mass ratio of 1-2:1-2 to obtain a mixed material with particles ≤ 2 mm;
[0011] S2. Preparation of aluminum raw materials:
[0012] (1) Pretreatment of coal gasification ash: drying the coal gasification ash to constant weight, dispersing and sieving through a ball mill to obtain coal gasification ash with a particle size of ≤2 mm and a particle size of 2 to 5 mm for later use;
[0013] (2) Lithium slag pretreatment: The lithium slag is dried to constant weight and dispersed into a particle size of ≤2 mm by a ball mill;
[0014] (3) mixing coal gasification ash slag with a particle size of ≤2 mm and lithium slag in a mass ratio of 1-2:1-2 to obtain a particle mixture with a particle size of ≤2 mm;
[0015] S3. Preparation of calcium raw materials:
[0016] (1) Alkali residue pretreatment: The papermaking sludge is placed in a sedimentation tank for preliminary standing, stratified, and the supernatant is removed. The obtained precipitate is rinsed three times with tap water, and the water is removed after each washing. Finally, it is filtered to reduce its water content to 20-30%, and then it is broken into small pieces, dried to constant weight, and crushed into particles ≤2 mm by a crusher for later use;
[0017] (2) Pretreatment of calcium-silicon slag: The calcium-silicon slag is piled up and air-dried to make its moisture content less than 15-25%, dried to constant weight, and crushed to particles ≤ 2 mm by a crusher for later use;
[0018] (3) mixing alkaline slag with a particle size of ≤2 mm and calcium-silicon slag in a mass ratio of 2-4:1-3 to obtain a mixed material with particles of ≤2 mm;
[0019] S4. Purification of sea sand: The sea sand washed with fresh water is piled up in a cool place to dry to obtain purified sea sand;
[0020] S5. Pretreatment of phosphogypsum: Dry the phosphogypsum to constant weight and grind it to a specific surface area of 300-500m 2 / kg, to obtain powder 1;
[0021] S6. Pretreatment of waste vitex and waste fir branches: the peeled and chopped waste vitex and waste fir branches are respectively dried by blast drying to a moisture content of ≤10%, then placed in a retort for carbonization, crushed in a crusher to a particle size of ≤2 mm, and then the waste vitex and waste fir branch particles are mixed at a mass ratio of 1-4:1-3 to obtain a carbon particle mixture of ≤2 mm;
[0022] S7, pressing and molding: Mix the S1 mixture, S2 mixture, S3 mixture, purified sea sand in S4, and powder 1 in S5 to obtain a mixed material, add 5-8% by weight of carbon particles to the mixed material, grind it to a specific surface area of 300-500m2 with a ball mill, 2 / kg, transfer to a mortar mixer, add 7-11% water by mass of the mixed material, mix evenly, put the mixed material into a mold, press into a cake, and dry;
[0023] S8, high temperature calcination: calcining the cake dried in step S7 at high temperature, cooling after calcination to obtain a high temperature calcined product;
[0024] S9, pretreatment of low carbon powder 2: crush the high temperature calcined product in step S8 into particles ≤ 2 mm by a crusher, and then grind it into a ball mill to a specific surface area of 450-550 m 2 / kg, and obtain low-carbon powder 2;
[0025] S10, preparation of plant ash: naturally air-dried rape straw is cut into 3-6 cm pieces, and then placed in a combustion furnace, with the thickness of the rape straw being ≤20 cm, and the upper layer is covered with coal gasification ash with a particle size of 2-5 mm in S2, and rape straw and coal gasification ash particles are alternately stacked, and repeated 2-3 times, while ensuring that there is a 10 cm gap between the top coal gasification ash straw particles and the top of the combustion furnace, and then calcined, and then the cooled calcined material is placed in a ball mill and ground to 600-800 m 2 / kg; obtain powder 3;
[0026] S11. Pretreatment of coarse aggregate:
[0027] (1) Pretreatment of waste aerated concrete: the cut waste aerated concrete is dried to constant weight, placed in a medium-free ball mill, and ground to obtain waste aerated concrete aggregate with a particle size of 5 to 20 mm, and then placed in a 10% by mass liquid paraffin solution and soaked for 20 to 40 minutes, and then the soaked aerated concrete is dried to constant weight;
[0028] (2) Waste rock pretreatment: The waste rock after impurities are removed is dried to constant weight, crushed to a particle size of 10 to 25 mm by a crusher, and then placed in a medium-free ball mill to grind waste rock aggregate with a particle size of 5 to 20 mm;
[0029] (3) mixing the waste aerated concrete and the waste rock aggregate in a mass ratio of 60-70%:30-40% to obtain a coarse aggregate for concrete;
[0030] S12. Preparation of water reducing agent:
[0031] (1) Bagasse pretreatment: The bagasse is dried to constant weight, 11% kerosene and 96% concentrated sulfuric acid are mixed in a volume ratio of 2-3:1 to obtain a mixed solution, 25-30% bagasse by mass of the mixed solution is added, and the mixture is soaked for 3-5 hours, cooled to room temperature, and the separated solvent is neutralized with a 25%-28% NaOH solution to a pH of 7-9, filtered, and a bagasse extract is obtained;
[0032] (2) Pretreatment of tofu wastewater: Stainless steel slag is added to the refrigerated tofu wastewater for flocculation treatment for 4 to 6 hours, and then filtered to obtain tofu wastewater filtrate;
[0033] (3) Preparation of water reducing agent: the pretreated bagasse extract and tofu wastewater filtrate are mixed in a volume ratio of 1-2:1-2 to prepare a water reducing agent;
[0034] S13, the preparation of sticky yellow rice slurry: the sticky yellow rice from which impurities are removed is dried to a moisture content of <0.2%, crushed to a particle size of <3 mm by a crusher, and boiled over low heat for 3 to 5 h with water, cooled to room temperature, filtered, and obtained a sticky yellow rice mixed slurry, which is stored in a refrigerator for standby use;
[0035] S14, concrete preparation: the powder 1 in S5, the low-carbon powder 2 in S9, and the powder 3 in S10 are mixed to obtain powder 4; then the powder 4 and the purified sea sand in S4 and the coarse aggregate in S11 are uniformly mixed to obtain powder 5, 7-13% sticky yellow rice slurry of the mass of powder 4 is added to the powder 5, and then 0.1-0.3% water reducing agent of the mass of powder 4 is added, and the mixture is stirred evenly, and lightweight concrete is obtained by pouring, demoulding and curing.
[0036] Optionally, the carbonization treatment in step S6 is carbonization for 3 to 6 hours in high temperature flue gas at 500 to 700°C.
[0037] Optionally, in step S7, the S1 mixture, the S2 mixture, the S3 mixture, the purified sea sand in S4, and the powder 1 in S5 are mixed in a weight ratio of 5-10%: 5-8%: 50-60%: 20-30%: 3-5% to obtain a mixed material.
[0038] Optionally, the pressure of the pressing in step S7 is 15-25 MPa, and the pressed molded body is a cake with a thickness of 2-4 cm and a diameter of 5-8 cm.
[0039] Optionally, the high temperature calcination in step S8 is to increase the temperature from room temperature to 700°C at a heating rate of 5°C / min, and then keep it warm for 20 minutes; then increase the temperature from 700°C to 1100-1200°C at a heating rate of 10°C / min, and then keep it warm for 20-50 minutes.
[0040] Optionally, the cooling in step S8 is rapid cooling by blowing air, cooling to room temperature at a wind speed of 50°C / min.
[0041] Optionally, the calcination in step S10 is: heating to 500° C. to 700° C. at a heating rate of 10 to 15° C. / min, and keeping the temperature for 3 to 5 hours.
[0042] Optionally, the soaking temperature of bagasse in step S12 is 45-55°C.
[0043] Optionally, during the cooking process in step S13, the mass concentration of sticky yellow rice is maintained at 4-10%.
[0044] Optionally, in step S14, the powder 1 in S5, the low-carbon powder 2 in S9, and the powder 3 in S10 are mixed in a mass ratio of 5-10%:80-90%:5-10% to obtain powder 4; the powder 4 is evenly mixed with the purified sea sand in S4 and the coarse aggregate in S11 in a mass ratio of 50-70%:15-30%:10-35% to obtain powder 5.
[0045] Beneficial effects of the present invention
[0046] (1) The coal gasification slag-lithium slag-steel slag based lightweight concrete of the present invention has the advantages of good volume stability, good physical properties, good working performance, good mechanical properties, etc., which greatly reduces the production cost, broadens the way of solid waste resource utilization, improves the mechanical properties, working performance and compatibility with admixtures of high-performance lightweight waste-utilizing concrete, and can realize efficient and scientific stable control of the production process of high-performance lightweight waste-utilizing concrete.
[0047] (2) The present invention utilizes 100% solid waste to prepare high-performance lightweight waste-utilizing concrete. The solid waste used in the preparation includes: cyanide tailings, steel slag, coal gasification ash slag, lithium slag, alkali slag, silica-calcium slag, phosphogypsum, stainless steel slag, sea sand, waste aerated concrete, waste stone, sugarcane bagasse, etc. The physical properties, working performance, and mechanical properties of the all-solid waste lightweight concrete of the present invention are improved compared with the index requirements in the "Technical Standard for the Application of Lightweight Aggregate Concrete" JGJ / T 12-2019. Its radioactivity meets the test index requirements in the "Limits of Radioactive Nuclides in Building Materials" GB 6566-2010, and its safety meets the requirements of the "Groundwater Quality Standard" GB / T 14848-2017. The present invention improves the utilization rate of solid waste raw materials, can significantly reduce the production cost of enterprises, and has significant economic and social environmental benefits.
[0048] (3) The coal gasification slag-lithium slag-steel slag-based lightweight concrete of the present invention utilizes low-carbon powder prepared from nonferrous metallurgical solid waste, chemical solid waste, steel solid waste, coal-based solid waste, agricultural solid waste, etc., and combines the mineral composition and content characteristics of the new low-carbon cement clinker to replace the silicate cement clinker; utilizes chemical solid waste (alkali slag, silica-calcium slag) to replace all calcium raw materials limestone; utilizes purified sea sand as high-silica raw material to replace traditional siliceous raw materials, coal-based solid waste (coal gasification ash and lithium slag) as aluminum raw material, steel solid waste (cyanide tailings, steel slag) as iron raw material, and chemical solid waste (phosphogypsum) as sulfur raw material. The synergistic effect between the multi-source solid wastes makes the composition of the high-performance lightweight waste-utilizing concrete more scientific and standardized, and more suitable for the actual production process;
[0049] (4) The present invention uses a specific crystal phase structure design to regulate the crystal phase structure, so that the low-carbon powder made from the high-temperature calcined product can have higher physical and mechanical properties in a short time, which is significantly better than the existing common Portland cement clinker of the same type; at the same time, the low-carbon powder of the present invention also has the excellent characteristics of significantly high strength, rapid setting, rapid hardening, low carbon, low alkali, and low chloride ion content. It can shorten the construction period, which is of great significance for the emergency construction and repair of municipal engineering, building decoration, road and bridge repair, and as a material and wartime emergency reserve technology.
[0050] (5) In the process of preparing low-carbon powder using calcium materials (alkali slag and calcium-silicon slag), silicon materials (purified sea sand), ferroaluminum materials (cyanide tailings, stainless steel slag, coal gasification ash slag and lithium slag) and sulfur materials (phosphogypsum) as raw materials, the present invention reasonably controls the particle size, molding conditions, calcination time and insulation time to form the best match among the four parameters and exert synergistic conditions, so that the low-carbon powder can form a specific crystalline phase structure, achieve excellent early, middle and late performance of the powder, and can replace silicate cement clinker.
[0051] (6) The low-carbon powder prepared by the present invention has a significant carbon reduction effect. The carbonaceous particles fired by discarded peach branches and discarded pear branches are mixed into the low-carbon powder, so that the firing temperature can be reduced by 100°C compared with silicate cement clinker, and the energy consumption is reduced by more than 10%. At the same time, all solid waste raw materials are used in the firing process of the low-carbon powder, and limestone is not used. CO2 emissions are reduced by more than 20%, which can significantly reduce the production cost of the enterprise and has good economic and social ecological environmental benefits.
[0052] (7) The present invention can purposefully and stably control the composition and content ratio of each mineral in the powder, and its performance is excellent, which can reach and exceed the existing silicate cement clinker. It is expected to be widely used and replace traditional silicate cement in large quantities, thus promoting the low-carbon sustainable development of the cement industry.
[0053] (8) The raw materials of the cementitious materials in the coal gasification slag-lithium slag-steel slag-based lightweight concrete of the present invention are low-carbon powder, phosphogypsum and plant ash. The three raw materials form the best match and exert synergistic conditions, so that the cementitious materials can form specific hydration products. Through the adsorption, bridging, cross-linking and dynamic reconstruction of the hydration products, the harmful ions in the raw materials are solidified and controlled, which provides a guarantee for the application of lightweight waste-recycling concrete in engineering. At the same time, the cementitious materials have excellent early, middle and late performance, and low water demand, which provides a guarantee for the physical and mechanical properties of the cementitious materials. The 7d and 28d activity indexes of the cementitious materials are respectively greater than 104% and greater than 102%, and other performance indicators meet the standard requirements of T / CECS 689-2020 "Technical Specifications for the Application of Solid Waste-Based Cementitious Materials".
[0054] (9) The wood ash in the cementitious material of the present invention is light in weight and alkaline, and can play the role of alkali excitation, and can also play the role of volcanic ash effect, while the inactive fine particles of coal gasification ash can play the role of micro-aggregate for the filling material system; after the waste aerated concrete and waste rock are surface-modified by a medium-free ball mill, the required slurry and water requirements of the system can be reduced in the lightweight waste-utilizing concrete; the sticky yellow rice mixed slurry can enhance the stability of the concrete in the concrete system through adsorption, bridging and cross-linking, and provide a guarantee for the working performance and mechanical properties of the lightweight waste-utilizing concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 The XRD patterns of the products calcined at different holding times in Example 2-S8;
[0056] Figure 2 The f-CaO content of the high temperature calcined product at different holding times in Example 2-S8;
[0057] Figure 3 XRD patterns of high temperature calcined products under different cooling methods in Example 2-S8;
[0058] Figure 4 This is a SEM image of the high temperature calcined product of Example 2-S8 after calcination at 1150°C, keeping the temperature for 30 minutes, and rapid cooling with air blowing;
[0059] Figure 5 for Figure 4 A magnified image of
[0060] Figure 6 This is the DES graph of the high temperature calcined product of Example 2-S8 after calcination at 1150°C, keeping warm for 30 minutes, and rapid cooling with air blowing;
[0061] Figure 7 is the mortar compressive strength of powder 2 in Example 2-S9;
[0062] Figure 8 The XRD patterns of the hydration products of powder 4 at different ages in Example 2-S14;
[0063] Fig. 9 The SEM images of the hydration products of powder 4 at different ages in Example 2-S14 are (A1), (A2)-3d, (B1), (B2)-7d, (C1), (C2)-28d;
[0064] Fig.10 DTA-TG curves of the pure slurry of powder 4 at different ages in Example 2-S14 (a)-3d, (b)-28d;
[0065] Fig.11 It is the DTA-TG curve of the pure slurry of powder 4 at different ages in Example 2-S14. DETAILED DESCRIPTION
[0066] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0067] Example 1
[0068] A method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete, the preparation method comprising the following steps:
[0069] S1. Cyanide tailings / steel slag pretreatment: First, the cyanide tailings and steel slag are dried to constant weight, crushed to ≤2mm particles by a crusher, and then the cyanide tailings and steel slag are mixed at a mass ratio of 2:1 to obtain a ≤2mm particle mixture;
[0070] S2. Preparation of aluminum raw materials:
[0071] (1) Pretreatment of coal gasification ash: drying the coal gasification ash to constant weight, dispersing and sieving through a ball mill to obtain coal gasification ash with a particle size of ≤2 mm and a particle size of 2 to 5 mm for later use;
[0072] (2) Lithium slag pretreatment: The lithium slag is dried to constant weight and dispersed into a particle size of ≤2 mm by a ball mill;
[0073] (3) mixing coal gasification ash slag with a particle size of ≤2 mm and lithium slag in a mass ratio of 2:1 to obtain a particle mixture with a particle size of ≤2 mm;
[0074] S3. Preparation of calcium raw materials:
[0075] (1) Alkali residue pretreatment: The papermaking sludge is placed in a sedimentation tank for preliminary standing, stratified, and the supernatant is removed. The obtained precipitate is rinsed three times with tap water, and the water is removed after each washing. Finally, it is filtered to reduce its water content to 20-30%, and then it is broken into small pieces, dried to constant weight, and crushed into particles ≤2 mm by a crusher for later use;
[0076] (2) Pretreatment of calcium-silicon slag: The calcium-silicon slag is piled up and air-dried to make its moisture content less than 15-25%, dried to constant weight, and crushed to particles ≤ 2 mm by a crusher for later use;
[0077] (3) mixing alkaline slag with a particle size of ≤2 mm and calcium-silicon slag in a mass ratio of 4:1 to obtain a mixed material with particles of ≤2 mm;
[0078] S4. Purification of sea sand: The sea sand washed with fresh water is piled up in a cool place to dry to obtain purified sea sand;
[0079] S5. Pretreatment of phosphogypsum: Dry the phosphogypsum to constant weight and grind it to a specific surface area of 300-500m 2 / kg, to obtain powder 1;
[0080] S6. Pretreatment of waste vitex and waste fir branches: the peeled and chopped waste vitex and waste fir branches are respectively dried by blast drying to a moisture content of ≤10%, then placed in high-temperature flue gas at 500°C for carbonization for 6 hours, crushed in a crusher to a particle size of ≤2 mm, and then the waste vitex and waste fir branch particles are mixed at a mass ratio of 1:3 to obtain a carbon particle mixture of ≤2 mm;
[0081] S7, pressing and molding: S1 mixture, S2 mixture, S3 mixture, purified sea sand in S4, and powder 1 in S5 are mixed in a weight ratio of 5%:5%:56%:30%:4% to obtain a mixture, 5% by weight of carbon particles are added to the mixture, and the mixture is ground to a specific surface area of 300-500m2 by a ball mill. 2 / kg, transfer to a mortar mixer, add 7% water by mass of the mixed material, mix evenly, put the mixed material into a mold, press at a pressure of 15MPa to obtain a shaped body with a thickness of 2cm and a diameter of 8cm, and dry;
[0082] S8, high temperature calcination: the cake dried in step S7 is subjected to high temperature calcination, the calcination system is: from room temperature to 700°C, the heating rate is 5°C / min, and then the temperature is kept for 20min; then from 700°C to 1100°C, the heating rate is 10°C / min, and then the temperature is kept for 50min; after the calcination is completed, it is cooled to obtain a high temperature calcined product;
[0083] S9, pretreatment of low carbon powder 2: crush the high temperature calcined product in step S8 into particles ≤ 2 mm by a crusher, and then grind it into a ball mill to a specific surface area of 450-550 m 2 / kg, and obtain low-carbon powder 2;
[0084] S10, preparation of plant ash: naturally air-dried rape straw is cut into 3-6 cm pieces, and then placed in a combustion furnace, with the thickness of the rape straw being ≤20 cm, and the upper layer is covered with coal gasification ash with a particle size of 2-5 mm in S2, and rape straw and coal gasification ash particles are alternately stacked, and repeated 2-3 times, while ensuring that there is a 10 cm gap between the top coal gasification ash straw particles and the top of the combustion furnace, and then calcined (at a heating rate of 10°C / min, heated to 700°C, and kept warm for 3 hours), and then the cooled calcined material is placed in a ball mill and ground to 600-800 m 2 / kg; obtain powder 3;
[0085] S11. Pretreatment of coarse aggregate:
[0086] (1) Pretreatment of waste aerated concrete: The cut waste aerated concrete is dried to constant weight, placed in a medium-free ball mill, and ground to obtain waste aerated concrete aggregate with a particle size of 5 to 20 mm, and then placed in a 10% mass fraction liquid paraffin solution and soaked for 20 minutes, and then the soaked aerated concrete is dried to constant weight;
[0087] (2) Pretreatment of waste rock: The waste rock after impurities are removed is dried to constant weight, crushed to a particle size of 10 to 25 mm by a crusher, and then placed in a medium-free ball mill to grind waste rock aggregate with a particle size of 5 to 20 mm;
[0088] (3) mixing the waste aerated concrete and the waste rock aggregate in a mass ratio of 70%:30% to obtain a coarse aggregate for concrete;
[0089] S12. Preparation of water reducing agent:
[0090] (1) Bagasse pretreatment: The bagasse was dried to constant weight, 11% kerosene and 96% concentrated sulfuric acid were mixed in a volume ratio of 2:1 to obtain a mixed solution, 25% bagasse by mass of the mixed solution was added, and the mixture was immersed at 45°C for 5 hours, cooled to room temperature, and the separated solvent was neutralized with 25% NaOH solution to pH 7, filtered, and obtained a bagasse extract;
[0091] (2) Pretreatment of tofu wastewater: Stainless steel slag was added to the refrigerated tofu wastewater for flocculation treatment for 4 h, and then filtered to obtain the tofu wastewater filtrate;
[0092] (3) Preparation of water reducing agent: The pretreated bagasse extract and tofu wastewater filtrate were mixed in a volume ratio of 1:1 to prepare a water reducing agent;
[0093] S13, the preparation of sticky yellow rice slurry: the sticky yellow rice with impurities removed is dried to moisture <0.2%, crushed to a particle size <3mm by a crusher, and boiled for 3-5h over a slow fire with water, and the sticky yellow rice mass concentration is kept at 4% during the boiling, cooled to room temperature, and obtained a sticky yellow rice mixed slurry after filtering, and stored refrigerated for standby use;
[0094] S14, concrete preparation: powder 1 in S5, low carbon powder 2 in S9, and powder 3 in S10 are mixed in a mass ratio of 10%:80%:10% to obtain powder 4; powder 4 and purified sea sand in S4 and coarse aggregate in S11 are evenly mixed in a mass ratio of 60%:30%:10% to obtain powder 5, 7% sticky yellow rice slurry of powder 4 by mass is added to powder 5, and then 0.1% water reducing agent of powder 4 by mass is added, the mixture is stirred evenly, and lightweight concrete is obtained by pouring, demoulding, and curing.
[0095] The chemical composition of powder 2 obtained in step S9 in Example 1 (see Table 1), the activity index of powder 4 in S14 (see Table 2), other performance indicators and test methods of powder 4 (see Table 3), the radioactivity test results of powder 5 (see Table 4), the technical indicators of all-solid waste lightweight concrete (see Table 5), and the 28d ion leaching of all-solid waste lightweight concrete (see Table 6).
[0096] Table 1 Chemical composition of powder 2 in Example 1-S9
[0097]
[0098] Table 2 Activity index of powder 4 in Example 1-S14
[0099]
[0100] Table 3 Other performance indicators and test methods of powder 4 in Example 1-S14
[0101]
[0102] 2: Technical indicators of "Technical Specifications for Application of Solid Waste-Based Cementitious Materials" T / CECS 689-2020.
[0103] Table 4 Radioactivity test results of concrete mixture in Example 1-S14
[0104]
[0105]
[0106] 3: It is the test index requirement in "Limits of Radioactive Nuclides in Building Materials" GB6566-2010.
[0107] Table 5 Technical indicators of lightweight concrete in Example 1-S14
[0108]
[0109]
[0110] 4: It is the test index requirement in "Technical Standard for Application of Lightweight Aggregate Concrete" JGJ / T 12-2019.
[0111] Table 6 Ion leaching of lightweight concrete in Example 1-S14 at 28 days (μg / L)
[0112]
[0113] 5: Technical indicators refer to Groundwater Quality Standard GB / T 14848-2017.
[0114] Example 2
[0115] A method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete, the preparation method comprising the following steps:
[0116] S1. Cyanide tailings / steel slag pretreatment: First, the cyanide tailings and steel slag are dried to constant weight, crushed to particles ≤ 2 mm by a crusher, and then the cyanide tailings and steel slag are mixed at a mass ratio of 1:1 to obtain a mixed material with particles ≤ 2 mm;
[0117] S2. Preparation of aluminum raw materials:
[0118] (4) Pretreatment of coal gasification ash: drying the coal gasification ash to constant weight, dispersing and sieving through a ball mill to obtain coal gasification ash with a particle size of ≤2 mm and a particle size of 2 to 5 mm for later use;
[0119] (5) Lithium slag pretreatment: The lithium slag is dried to constant weight and dispersed into a particle size of ≤2 mm by a ball mill;
[0120] (6) mixing coal gasification ash slag with a particle size of ≤2 mm and lithium slag in a mass ratio of 1:1 to obtain a particle mixture with a particle size of ≤2 mm;
[0121] S3. Preparation of calcium raw materials:
[0122] (1) Alkali residue pretreatment: The papermaking sludge is placed in a sedimentation tank for preliminary standing, stratified, and the supernatant is removed. The obtained precipitate is rinsed three times with tap water, and the water is removed after each washing. Finally, it is filtered to reduce its water content to 20-30%, and then it is broken into small pieces, dried to constant weight, and crushed into particles ≤2 mm by a crusher for later use;
[0123] (2) Pretreatment of calcium-silicon slag: The calcium-silicon slag is piled up and air-dried to make its moisture content less than 15-25%, dried to constant weight, and crushed to particles ≤ 2 mm by a crusher for later use;
[0124] (3) mixing alkaline slag with a particle size of ≤2 mm and calcium-silicon slag in a mass ratio of 2:1 to obtain a mixed material with particles of ≤2 mm;
[0125] S4. Purification of sea sand: The sea sand washed with fresh water is piled up in a cool place to dry to obtain purified sea sand;
[0126] S5. Pretreatment of phosphogypsum: Dry the phosphogypsum to constant weight and grind it to a specific surface area of 300-500m 2 / kg, to obtain powder 1;
[0127] S6. Pretreatment of waste vitex and waste fir branches: the peeled and chopped waste vitex and waste fir branches are respectively dried by blast drying to a moisture content of ≤10%, then placed in a high-temperature flue gas at 600°C for carbonization for 5 hours, crushed to a particle size of ≤2 mm in a crusher, and then the waste vitex and waste fir branch particles are mixed at a mass ratio of 1:1 to obtain a carbon particle mixture of ≤2 mm;
[0128] S7, pressing and molding: S1 mixture, S2 mixture, S3 mixture, purified sea sand in S4, and powder 1 in S5 are mixed in a weight ratio of 10%:8%:50%:27%:5% to obtain a mixture, 6% by weight of carbon particles are added to the mixture, and the mixture is ground to a specific surface area of 300-500m2 by a ball mill. 2 / kg, transferred to a mortar mixer, added 8% water by mass of the mixed material, mixed evenly and put the mixed material into a mold, pressed at a pressure of 20MPa to obtain a shaped body with a thickness of 3cm and a diameter of 7cm, and dried;
[0129] S8, high temperature calcination: the cake dried in step S7 is subjected to high temperature calcination, the calcination system is: from room temperature to 700°C, the heating rate is 5°C / min, and then the temperature is kept for 20min; then from 700°C to 1150°C, the heating rate is 10°C / min, and then the temperature is kept for 30min; after the calcination is completed, it is cooled to obtain a high temperature calcined product;
[0130] S9, pretreatment of low carbon powder 2: crush the high temperature calcined product in step S8 into particles ≤ 2 mm by a crusher, and then grind it into a ball mill to a specific surface area of 450-550 m 2 / kg, and obtain low-carbon powder 2;
[0131] S10, preparation of plant ash: naturally air-dried rape straw is cut into 3-6 cm pieces, and then placed in a combustion furnace, with the thickness of the rape straw being ≤20 cm, and the upper layer is covered with coal gasification ash with a particle size of 2-5 mm in S2, and rape straw and coal gasification ash particles are alternately stacked, and repeated 2-3 times, while ensuring that there is a 10 cm gap between the top coal gasification ash straw particles and the top of the combustion furnace, and then calcined (at a heating rate of 12°C / min, heated to 600°C, and kept warm for 4 hours), and then the cooled calcined material is placed in a ball mill and ground to 600-800m 2 / kg; obtain powder 3;
[0132] S11. Pretreatment of coarse aggregate:
[0133] (1) Pretreatment of waste aerated concrete: The cut waste aerated concrete is dried to constant weight, placed in a medium-free ball mill, and ground to obtain waste aerated concrete aggregate with a particle size of 5 to 20 mm, and then immersed in a 10% mass fraction liquid paraffin solution for 30 minutes, and then the immersed aerated concrete is dried to constant weight;
[0134] (2) Waste rock pretreatment: The waste rock after impurities are removed is dried to constant weight, crushed to a particle size of 10 to 25 mm by a crusher, and then placed in a medium-free ball mill to grind waste rock aggregate with a particle size of 5 to 20 mm;
[0135] (3) mixing the waste aerated concrete and the waste rock aggregate in a mass ratio of 65%:35% to obtain a coarse aggregate for concrete;
[0136] S12. Preparation of water reducing agent:
[0137] (1) Bagasse pretreatment: The bagasse was dried to constant weight, 11% kerosene and 96% concentrated sulfuric acid were mixed at a volume ratio of 2.5:1 to obtain a mixed solution, 28% bagasse by mass of the mixed solution was added, and the mixture was soaked at 50° C. for 4 h, cooled to room temperature, and the separated solvent was neutralized with 26% NaOH solution to pH 8, filtered, and obtained a bagasse extract;
[0138] (2) Pretreatment of tofu wastewater: stainless steel slag was added to the refrigerated tofu wastewater for flocculation treatment for 5 h, and then filtered to obtain the tofu wastewater filtrate;
[0139] (3) Preparation of water reducing agent: The pretreated bagasse extract and tofu wastewater filtrate were mixed in a volume ratio of 1:2 to prepare a water reducing agent;
[0140] S13, the preparation of sticky yellow rice slurry: the sticky yellow rice with impurities removed is dried to moisture <0.2%, crushed to a particle size <3mm by a crusher, and boiled for 3-5h over a slow fire with water, and the sticky yellow rice mass concentration is kept at 8% during the boiling, cooled to room temperature, and obtained a sticky yellow rice mixed slurry after filtering, and stored refrigerated for standby use;
[0141] S14, concrete preparation: powder 1 in S5, low carbon powder 2 in S9, and powder 3 in S10 are mixed in a mass ratio of 10%:84%:6% to obtain powder 4; powder 4 and purified sea sand in S4 and coarse aggregate in S11 are mixed in a mass ratio of 50%:15%:35% to obtain powder 5, sticky yellow rice slurry of 10% by mass of powder 4 is added to powder 5, and then a water reducing agent of 0.2% by mass of powder 4 is added, the mixture is stirred evenly, and lightweight concrete is obtained by pouring, demoulding, and curing.
[0142] The chemical composition of powder 2 obtained in Example 2 (see Table 7), the activity index of powder 4 in S14 (see Table 8), other performance indicators and test methods of powder 4 (see Table 9), the radioactivity test results of powder 5 (see Table 10), the technical indicators of high-performance lightweight waste-utilizing concrete (see Table 11), and the 28d ion leaching of high-performance lightweight waste-utilizing concrete (see Table 12).
[0143] Table 7 Chemical composition of powder 2 in Example 2-S9
[0144]
[0145] Table 8 Activity index of powder 4 in Example 2-S14
[0146]
[0147] Table 9 Other performance indicators and test methods of powder 4 in Example 2-S14
[0148]
[0149]
[0150] 2: Technical indicators of "Technical Specifications for Application of Solid Waste-Based Cementitious Materials" T / CECS 689-2020.
[0151] Table 10 Radioactivity test results of concrete mixture in Example 2-S14
[0152]
[0153] 3: It is the test index requirement in "Limits of Radioactive Nuclides in Building Materials" GB6566-2010.
[0154] Table 11 Technical indicators of lightweight concrete in Example 2-S14
[0155]
[0156]
[0157] 4: It is the test index requirement in "Technical Standard for Application of Lightweight Aggregate Concrete" JGJ / T 12-2019.
[0158] Table 12 Ion leaching of lightweight concrete in Example 2-S14 at 28 days (μg / L)
[0159]
[0160] 5: Technical indicators refer to Groundwater Quality Standard GB / T 14848-2017.
[0161] Example 3
[0162] A method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete, the preparation method comprising the following steps:
[0163] S1. Cyanide tailings / steel slag pretreatment: First, the cyanide tailings and steel slag are dried to constant weight, crushed to ≤2mm particles by a crusher, and then the cyanide tailings and steel slag are mixed at a mass ratio of 1:2 to obtain a ≤2mm particle mixture;
[0164] S2. Preparation of aluminum raw materials:
[0165] (7) Pretreatment of coal gasification ash: drying the coal gasification ash to constant weight, dispersing and sieving through a ball mill to obtain coal gasification ash with a particle size of ≤2 mm and a particle size of 2 to 5 mm for later use;
[0166] (8) Lithium slag pretreatment: The lithium slag is dried to constant weight and dispersed into a particle size of ≤2 mm by a ball mill;
[0167] (9) mixing coal gasification ash slag with a particle size of ≤2 mm and lithium slag in a mass ratio of 1:2 to obtain a particle mixture with a particle size of ≤2 mm;
[0168] S3. Preparation of calcium raw materials:
[0169] (1) Alkali residue pretreatment: The papermaking sludge is placed in a sedimentation tank for preliminary standing, stratified, and the supernatant is removed. The obtained precipitate is rinsed three times with tap water, and the water is removed after each washing. Finally, it is filtered to reduce its water content to 20-30%, and then it is broken into small pieces, dried to constant weight, and crushed into particles ≤2 mm by a crusher for later use;
[0170] (2) Pretreatment of calcium-silicon slag: The calcium-silicon slag is piled up and air-dried to make its moisture content less than 15-25%, dried to constant weight, and crushed to particles ≤ 2 mm by a crusher for later use;
[0171] (3) mixing alkaline slag with a particle size of ≤2 mm and calcium-silicon slag in a mass ratio of 2:3 to obtain a mixed material with particles of ≤2 mm;
[0172] S4. Purification of sea sand: The sea sand washed with fresh water is piled up in a cool place to dry to obtain purified sea sand;
[0173] S5. Pretreatment of phosphogypsum: Dry the phosphogypsum to constant weight and grind it to a specific surface area of 300-500m 2 / kg, to obtain powder 1;
[0174] S6. Pretreatment of waste vitex and waste fir branches: the peeled and chopped waste vitex and waste fir branches are respectively dried by blast drying to a moisture content of ≤10%, then placed in a high-temperature flue gas at 700°C for carbonization for 3 hours, crushed in a crusher to a particle size of ≤2 mm, and then the waste vitex and waste fir branch particles are mixed at a mass ratio of 4:1 to obtain a carbon particle mixture of ≤2 mm;
[0175] S7, pressing and molding: Mix the S1 mixture, S2 mixture, S3 mixture, purified sea sand in S4, and powder 1 in S5 in a weight ratio of 10%:7%:60%:20%:3% to obtain a mixture, add 8% by weight of carbon particles to the mixture, grind it to a specific surface area of 300-500m2 with a ball mill, 2 / kg, transferred to a mortar mixer, added with 11% water by mass of the mixed material, mixed evenly and put into a mold, pressed at a pressure of 25MPa to obtain a shaped body with a thickness of 4cm and a diameter of 5cm, and dried;
[0176] S8, high temperature calcination: the cake dried in step S7 is subjected to high temperature calcination, the calcination system is: from room temperature to 700°C, the heating rate is 5°C / min, and then the temperature is kept for 20min; then from 700°C to 1200°C, the heating rate is 10°C / min, and then the temperature is kept for 20min; after the calcination is completed, it is cooled to obtain a high temperature calcined product;
[0177] S9, pretreatment of low carbon powder 2: crush the high temperature calcined product in step S8 into particles ≤ 2 mm by a crusher, and then grind it into a ball mill to a specific surface area of 450-550 m 2 / kg, and obtain low-carbon powder 2;
[0178] S10, preparation of plant ash: naturally air-dried rape straw is cut into 3-6 cm pieces, and then placed in a combustion furnace, with the thickness of the rape straw being ≤20 cm, and the upper layer is covered with coal gasification ash with a particle size of 2-5 mm in S2, and rape straw and coal gasification ash particles are alternately stacked, and repeated 2-3 times, while ensuring that there is a 10 cm gap between the top coal gasification ash straw particles and the top of the combustion furnace, and then calcined (at a heating rate of 15°C / min, heated to 500°C, and kept warm for 5h), and then the cooled calcined material is placed in a ball mill and ground to 600-800m 2 / kg; obtain powder 3;
[0179] S11. Pretreatment of coarse aggregate:
[0180] (4) Pretreatment of waste aerated concrete: The cut waste aerated concrete is dried to constant weight, placed in a medium-free ball mill, and ground to obtain waste aerated concrete aggregate with a particle size of 5 to 20 mm, and then immersed in a 10% mass fraction liquid paraffin solution for 40 minutes, and then the immersed aerated concrete is dried to constant weight;
[0181] (5) Pretreatment of waste rock: The waste rock after impurities are removed is dried to constant weight, crushed to a particle size of 10 to 25 mm by a crusher, and then placed in a medium-free ball mill to grind waste rock aggregate with a particle size of 5 to 20 mm;
[0182] (6) mixing the waste aerated concrete and the waste rock aggregate in a mass ratio of 60%:40% to obtain a coarse aggregate for concrete;
[0183] S12. Preparation of water reducing agent:
[0184] (1) Bagasse pretreatment: The bagasse was dried to constant weight, 11% kerosene and 96% concentrated sulfuric acid were mixed in a volume ratio of 3:1 to obtain a mixed solution, 30% bagasse by mass of the mixed solution was added, and the mixture was soaked at 55° C. for 3 h, cooled to room temperature, and the separated solvent was neutralized with 28% NaOH solution to a pH of 9, filtered, and obtained a bagasse extract;
[0185] (2) Pretreatment of tofu wastewater: stainless steel slag was added to the refrigerated tofu wastewater for flocculation treatment for 6 h, and then filtered to obtain the tofu wastewater filtrate;
[0186] (3) Preparation of water reducing agent: The pretreated bagasse extract and tofu wastewater filtrate were mixed in a volume ratio of 2:1 to prepare a water reducing agent;
[0187] S13, the preparation of sticky yellow rice slurry: the sticky yellow rice with impurities removed is dried to moisture <0.2%, crushed to a particle size <3mm by a crusher, and boiled for 3-5h over a slow fire with water, and the sticky yellow rice mass concentration is kept at 10% during the boiling, cooled to room temperature, and obtained a sticky yellow rice mixed slurry after filtering, and stored refrigerated for standby use;
[0188] S14, concrete preparation: powder 1 in S5, low carbon powder 2 in S9, and powder 3 in S10 are mixed in a mass ratio of 5%:90%:5% to obtain powder 4; powder 4 and purified sea sand in S4 and coarse aggregate in S11 are mixed in a mass ratio of 70%:15%:15% to obtain powder 5, 13% sticky yellow rice slurry of powder 4 by mass is added to powder 5, and then 0.3% water reducing agent of powder 4 by mass is added, the mixture is stirred evenly, and lightweight concrete is obtained by pouring, demoulding, and curing.
[0189] The chemical composition of powder 2 obtained by S9 in Example 3 (see Table 13), the activity index of powder 4 in S14 (see Table 14), other performance indicators and test methods of powder 4 (see Table 15), the radioactivity test results of powder 5 (see Table 16), the technical indicators of high-performance lightweight waste-utilizing concrete (see Table 17), and the 28d ion leaching of high-performance lightweight waste-utilizing concrete (see Table 18).
[0190] Table 13 Chemical composition of powder 2 in Example 3-S9
[0191]
[0192] Table 14 Activity index of powder 4 in Example 3-S14
[0193]
[0194] Table 15 Other performance indicators and test methods of powder 4 in Example 3-S14
[0195]
[0196] 2: Technical indicators of "Technical Specifications for Application of Solid Waste-Based Cementitious Materials" T / CECS 689-2020.
[0197] Table 16 Radioactivity test results of concrete mixture in Example 3-S14
[0198]
[0199] 3: It is the test index requirement in "Limits of Radioactive Nuclides in Building Materials" GB6566-2010.
[0200] Table 17 Technical indicators of lightweight concrete in Example 3-S14
[0201]
[0202] 4: It is the test index requirement in "Technical Standard for Application of Lightweight Aggregate Concrete" JGJ / T 12-2019.
[0203] Table 18 Ion leaching of lightweight concrete in Example 3-S14 at 28 days (μg / L)
[0204]
[0205] 5: Technical indicators refer to Groundwater Quality Standard GB / T 14848-2017.
[0206] The present invention will be further described below in conjunction with the accompanying drawings:
[0207] Composition, morphology and properties of the high temperature calcined product in step S8 of Example 2
[0208] Appropriate holding time is also crucial to the quality of high-temperature calcination at room temperature. Therefore, the raw materials of the cake in S8 were kept at 1150℃ for 20min, 30min, 40min, and 50min respectively, and then quickly cooled. The mineral composition and f-CaO content of the clinker were analyzed to explore the effect of holding time on the sintering products of the system. The mineral composition and f-CaO content under different holding times were measured, and the results are as follows: Figure 1 and Figure 2 shown.
[0209] Depend on Figure 1 It can be seen that the main mineral composition of the high-temperature calcined product prepared is β-C2S, C4AF and CaSO4. When the holding time is less than 30min, the high temperature calcined product is β-C2S, C4AF and CaSO4 are the main components, and as the insulation time increases The intensity of the β-C2S diffraction peak gradually increased, while the intensity of the CaSO4 diffraction peak decreased, indicating that extending the holding time is beneficial to the mineral content of the high-temperature calcined product. The formation of β-C2S; when the holding time is more than 30min, the sintered product is β-C2S is the main component, and as the insulation time increases, The intensity of the β-C2S diffraction peak gradually decreases, and the CaSO4 diffraction peak is no longer observed, indicating that the products have begun to decompose. Too long a holding time is not necessarily beneficial to the formation of minerals in the high-temperature calcined product. It can be seen that the holding time of the high-temperature calcined product is 20 to 50 minutes, and the most suitable holding time is 30 minutes.
[0210] from Figure 2 It can be seen that the holding time has a certain influence on the f-CaO content in the high-temperature calcination product system. With the extension of the holding time, the f-CaO content in the clinker system has a tendency to decrease first and then increase. When the holding time is 30 minutes, the f-CaO content is as low as 0.88%. When the holding time is greater than 30 minutes, the f-CaO content increases because f-CaSO4 is partially decomposed. It can be seen that when the holding time is too short, the reaction is not complete, and too long a holding time will cause f-CaSO4 to decompose into CaO and SO3, affecting its mineral composition. Therefore, combined with the above analysis of the f-CaO content, the appropriate holding time is determined to be 30 minutes.
[0211] The cooling method has a great influence on the crystal transformation of the high-temperature calcined product mineral C2S. Therefore, two cooling methods, namely, rapid cooling by air blowing and natural cooling at room temperature (26±2)℃, were designed. The mixture was fired at a firing temperature of 1150℃ and a holding time of 30min. The appropriate cooling method was determined by analyzing the product composition under the two cooling methods. The results are shown in Figure 2. Figure 3 As shown. Figure 3 It can be seen that the sintering products of the two cooling methods are relatively consistent. The main components are β-C2S, C4AF and CaSO4. No transformation from β-C2S to γ-C2S was found in the high temperature calcined product after natural cooling at room temperature (26±2)℃. The intensity of the diffraction peak decreased significantly, which may be due to the slow cooling speed. The high temperature calcined product still maintained a high temperature for a long time after leaving the furnace. It can be seen that the cooling method of the high-temperature calcined product can be either rapid cooling by blowing air or natural cooling at room temperature (26±2)℃, and the best cooling method is rapid cooling by blowing air.
[0212] Figure 4 This is a SEM image of the high temperature calcined product of Example 2-S8 after calcination at 1150°C, keeping the temperature for 30 minutes, and rapid cooling with air blowing; Figure 5 for Figure 4 A magnified image of Figure 6 This is the DES graph of the high temperature calcined product of Example 2-S8 after calcination at 1150°C, keeping warm for 30 minutes, and rapid cooling by blowing. Figure 4 , Figure 5 Most of the products are in the form of oval particles with a particle size of more than 10μm. The mineral particles are tightly combined, which is not only convenient for grinding, but also has better hydration performance due to the relatively large specific surface area of the mineral particles. Figure 5 EDS analysis was performed on point 1, and the element statistics are shown in Table 19. The mineral at point 1 is C2S, and a small amount of Al, S, Mg, Na and K enter the C2S lattice. The impurity elements entering the lattice can stabilize C2S in the β form and improve its hydration reaction activity.
[0213] Table 19 Figure 4 Statistical results of EDS analysis at one point (mol%)
[0214]
[0215] An appropriate amount of gypsum was added to the powder 2 prepared by high temperature calcination product in Example 2, and the mortar strength test was carried out at a water-cement ratio of 0.5 and a sand-cement ratio of 3. The benchmark cement was used as a comparative sample, and the mortar compressive strength test was carried out at the same water-cement ratio and sand-cement ratio. The compressive strength was measured at the age of 1d, 3d, 7d, 28d, and 90d, and the mortar strength of the benchmark cement and the powder 2 was obtained as follows: Figure 7 As shown. It can be seen from the figure that the 1d and 3d compressive strengths of the cement prepared with powder 2 are significantly higher than those of the benchmark cement. Usually, the strength level of the benchmark cement at 7d can be reached at 3d. The 28d strength of the cement prepared with powder 2 is equivalent to that of the benchmark cement, and as the curing age increases, the 90d strength can exceed that of the benchmark cement. The strength performance of powder 2 depends on the optimized matching relationship of various minerals in its system, which can effectively ensure the optimal ratio of several minerals in powder 2, ensure the coordinated hydration between minerals, and promote the stable performance of the strength performance of powder 2. Furthermore, the performance of powder 2 is similar to or even better than that of silicate cement clinker, indicating that powder 2 can replace traditional silicate cement on a large scale.
[0216] Composition and morphology of the hydration product of the powder material 4 for lightweight concrete in step S14 of Example 2
[0217] The properties of the paste after hydration and hardening of silicate cement mainly depend on the hydration products of C3S and C3A. The equation of the hydration reaction process is as follows:
[0218] 3CaO·SiO2+nH2O=xCaO·SiO2·yH2O+(3-x)Ca(OH)2 (1)
[0219] The main hydration products are CSH gel and Ca(OH)2. The hydration reaction process of C2S is similar to that of C3S. The hydration reaction of C3A is rapid, and the reaction formula is as follows:
[0220] 3CaO·Al2O3+6H2O=3CaO·Al2O3·6H2O (2)
[0221] When the concentration of Ca(OH)2 in the liquid phase reaches saturation, the hydration reaction can also be carried out according to the following formula:
[0222] 3CaO·Al2O3+Ca(OH)2+12H2O=4CaO·Al2O3·13H2O (3)
[0223] Under the condition of gypsum participating in the reaction
[0224] 4CaO·Al2O3·13H2O+3(CaSO4·2H2O)+14H2O=
[0225] 3CaO·Al2O3·3CaSO4·32H2O+Ca(OH)2(4)
[0226] 3CaO·Al2O3·3CaSO4·32H2O is trisulfur hydrated calcium sulfoaluminate, also known as ettringite (AFt). The C4AF reaction is similar to it, and the Al in AFt can be replaced by Fe.
[0227] therefore, Figure 8 The XRD patterns of the hydration products of powder 4 at different ages in Example 2-S14 are shown in Table 1. Figure 8 It can be seen that the hydration products generated by the hardened slurry of powder 4 at each curing age include: AFt, Ca(OH)2, amorphous CSH gel, and unreacted C3S and C2S. With the extension of the curing age, the content of AFt and Ca(OH)2 gradually increases, while the content of C3S and C2S gradually decreases. Since CSH gel is an amorphous substance, it is almost impossible to identify it in the XRD spectrum. In the figure, the "mantou peak" protrusion of 25° to 35° indicates the existence of amorphous substances.
[0228] Fig. 9 The microscopic morphology of the hardened slurry of powder 4 at different ages. Fig. 9 It can be seen from (A1) and (A2) that a large number of reaction products have been generated in the hardened paste with a hydration age of 3 days. A large number of CSH gels and AFt crystals are intertwined with each other, and the network structure of the hardened paste is basically formed, which makes the concrete have a high strength at an early stage. Fig. 9 As can be seen from (B1) and (B2), at the age of 7 days, a large amount of calcium sulfonate has been produced in the system, and the grain size of calcium sulfonate has also increased significantly. The calcium sulfonate with relatively high crystallinity needs to be further intertwined, and the CSH gel in the system fills the pores, making the system more compact. When the hydration age is 28 days (see Figures (C1) and (C2)), with the large amount of hydration products generated, the gel completely wraps the calcium sulfonate crystals, the pores in the system are reduced, and the structure becomes more compact. The synergistic generation of calcium sulfonate and CSH gel in the system effectively promotes the growth of the strength of the concrete system.
[0229] Fig.10 This is the DTA-TG comparison chart of the pure slurry of powder 4 in S14 after hydration for 3d and 28d. Fig.10 On the DTA-TG curves of (a) and 10(b), there are the following three common endothermic peaks and one exothermic valley in the temperature range below 1000℃: the endothermic peak at around 120℃ is the dehydration endothermic peak of CSH gel and AFt in the hydration product; the endothermic peak at around 460℃ corresponds to the decomposition of Ca(OH)2; the endothermic peak at around 695℃ is caused by the conversion of unhydrated β-C2S in powder 4 to α-C2S; the exothermic valley at around 882℃ is the formation of β-wollastonite by CSH.
[0230] Fig.11 This is the FT-IR comparison of the hydration of powder 4 in S14 for 3d, 7d, and 28d. It can be seen that the spectra of samples at different ages are similar, basically showing the same characteristic absorption bands, and each absorption peak moves toward the direction of small wave numbers. The wave number in the figure is 459cm -1The absorption peak at 795 cm is attributed to the bending vibration of Si-O bond. -1 The vibration absorption peaks of quartz are around 990cm -1 The absorption peak is caused by the asymmetric vibration of Si-O in the [SiO4] structure, which is the characteristic peak of CSH. The wave number is 1427cm -1 The absorption band is CO3 2- The asymmetric stretching vibration band is probably due to the carbonization of the sample. The wave number is 1645 cm -1 The absorption band at is attributed to the bending vibration of the OH bond in water. The wave number is 3425cm -1 The bands on the left and right are the stretching vibration bands of structural water in the hydration product CSH gel, indicating that CSH gel is continuously generated with the increase of age. -1 The absorption peak is not obvious. This is because the hydroxyl groups in AFt and CSH gels are not typical hydroxyl groups. They have no clear boundaries with the hydrogen bonds and molecular bonds in the crystal water, so they are overshadowed by the 3425cm -1 However, since most of the water in AFt is crystal water, the peak at 3425 cm -1 The absorption peak overlaps with the structural water of CSH, showing a strong absorption peak. -1 The strong absorption band at 1090cm belongs to the asymmetric stretching vibration of SO bond. Its vibration peak increases and sharpens with the extension of curing time. -1 There is an obvious absorption peak at 990cm, indicating that AFt has been generated after 3 days of hydration. A considerable amount of AFt has been formed after 3 days of hydration, which shows that the formation speed of AFt is quite fast, which is consistent with the analysis results. -1 and 1090cm -1 The absorption peaks of AFt and CSH gel reflect the rapid coordinated growth process at each age, which is consistent with Figure 8 The disappearance of the gypsum diffraction peak in the XRD pattern is consistent with that in the experiment.
[0231] In summary, the present invention uses solid waste to prepare coal gasification slag-lithium slag-steel slag based lightweight concrete, and its technical indicators such as physical and mechanical properties (working performance, mechanical properties) are improved compared with the requirements of the indicators in the "Technical Standard for the Application of Lightweight Aggregate Concrete" JGJ / T 12-2019, which is better than the existing products on the market and worthy of vigorous promotion.
[0232] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete, the preparation method comprising the following steps: S1. Cyanide tailings / steel slag pretreatment: First, the cyanide tailings and steel slag are dried to constant weight, crushed to particles ≤ 2 mm by a crusher, and then the cyanide tailings and steel slag are mixed at a mass ratio of 1-2:1-2 to obtain a mixed material with particles ≤ 2 mm; S2. Preparation of aluminum raw materials: (1) Pretreatment of coal gasification ash: drying the coal gasification ash to constant weight, dispersing and sieving through a ball mill to obtain coal gasification ash with a particle size of ≤2 mm and a particle size of 2 to 5 mm for later use; (2) Lithium slag pretreatment: The lithium slag is dried to constant weight and dispersed into a particle size of ≤2 mm by a ball mill; (3) mixing coal gasification ash slag with a particle size of ≤2 mm and lithium slag in a mass ratio of 1-2:1-2 to obtain a particle mixture with a particle size of ≤2 mm; S3. Preparation of calcium raw materials: (1) Alkali residue pretreatment: The papermaking sludge is placed in a sedimentation tank for preliminary standing, stratified, and the supernatant is removed. The obtained precipitate is rinsed three times with tap water, and the water is removed after each washing. Finally, it is filtered to reduce its water content to 20-30%, and then it is broken into small pieces, dried to constant weight, and crushed into particles ≤2 mm by a crusher for later use; (2) Pretreatment of calcium-silicon slag: The calcium-silicon slag is piled up and air-dried to make its moisture content less than 15-25%, dried to constant weight, and crushed to particles ≤ 2 mm by a crusher for later use; (3) mixing alkaline slag with a particle size of ≤2 mm and calcium-silicon slag in a mass ratio of 2-4:1-3 to obtain a mixed material with particles of ≤2 mm; S4. Purification of sea sand: The sea sand washed with fresh water is piled up in a cool place to dry to obtain purified sea sand; S5. Pretreatment of phosphogypsum: Dry the phosphogypsum to constant weight and grind it to a specific surface area of 300-500m 2 / kg, to obtain powder 1; S6. Pretreatment of waste vitex and waste fir branches: the peeled and chopped waste vitex and waste fir branches are respectively dried by blast drying to a moisture content of ≤10%, then placed in a retort for carbonization, crushed in a crusher to a particle size of ≤2 mm, and then the waste vitex and waste fir branch particles are mixed at a mass ratio of 1-4:1-3 to obtain a carbon particle mixture of ≤2 mm; S7, pressing and molding: Mix the S1 mixture, S2 mixture, S3 mixture, purified sea sand in S4, and powder 1 in S5 to obtain a mixed material, add 5-8% by weight of carbon particles to the mixed material, grind it to a specific surface area of 300-500m2 with a ball mill, 2 / kg, transfer to a mortar mixer, add 7-11% water by mass of the mixed material, mix evenly, put the mixed material into a mold, press into a cake, and dry; S8, high temperature calcination: calcining the cake dried in step S7 at high temperature, cooling after calcination to obtain a high temperature calcined product; S9, pretreatment of low carbon powder 2: crush the high temperature calcined product in step S8 into particles ≤ 2 mm by a crusher, and then grind it into a ball mill to a specific surface area of 450-550 m 2 / kg, and obtain low-carbon powder 2; S10, preparation of plant ash: naturally air-dried rape straw is cut into 3-6 cm pieces, and then placed in a combustion furnace, with the thickness of the rape straw being ≤20 cm, and the upper layer is covered with coal gasification ash with a particle size of 2-5 mm in S2, and rape straw and coal gasification ash particles are alternately stacked, and repeated 2-3 times, while ensuring that there is a 10 cm gap between the top coal gasification ash straw particles and the top of the combustion furnace, and then calcined, and then the cooled calcined material is placed in a ball mill and ground to 600-800 m 2 / kg; obtain powder 3; S11. Pretreatment of coarse aggregate: (1) Pretreatment of waste aerated concrete: the cut waste aerated concrete is dried to constant weight, placed in a medium-free ball mill, and ground to obtain waste aerated concrete aggregate with a particle size of 5 to 20 mm, and then placed in a 10% by mass liquid paraffin solution and soaked for 20 to 40 minutes, and then the soaked aerated concrete is dried to constant weight; (2) Waste rock pretreatment: The waste rock after impurities are removed is dried to constant weight, crushed to a particle size of 10 to 25 mm by a crusher, and then placed in a medium-free ball mill to grind waste rock aggregate with a particle size of 5 to 20 mm; (3) mixing the waste aerated concrete and the waste rock aggregate in a mass ratio of 60-70%:30-40% to obtain a coarse aggregate for concrete; S12. Preparation of water reducing agent: (1) Bagasse pretreatment: The bagasse is dried to constant weight, 11% kerosene and 96% concentrated sulfuric acid are mixed in a volume ratio of 2-3:1 to obtain a mixed solution, 25-30% bagasse by mass of the mixed solution is added, and the mixture is soaked for 3-5 hours, cooled to room temperature, and the separated solvent is neutralized with a 25%-28% NaOH solution to a pH of 7-9, filtered, and a bagasse extract is obtained; (2) Pretreatment of tofu wastewater: Stainless steel slag is added to the refrigerated tofu wastewater for flocculation treatment for 4 to 6 hours, and then filtered to obtain tofu wastewater filtrate; (3) Preparation of water reducing agent: the pretreated bagasse extract and tofu wastewater filtrate are mixed in a volume ratio of 1-2:1-2 to prepare a water reducing agent; S13, the preparation of sticky yellow rice slurry: the sticky yellow rice from which impurities are removed is dried to a moisture content of <0.2%, crushed to a particle size of <3 mm by a crusher, and boiled over low heat for 3 to 5 h with water, cooled to room temperature, filtered, and obtained a sticky yellow rice mixed slurry, which is stored in a refrigerator for standby use; S14, concrete preparation: the powder 1 in S5, the low-carbon powder 2 in S9, and the powder 3 in S10 are mixed to obtain powder 4; then the powder 4 and the purified sea sand in S4 and the coarse aggregate in S11 are uniformly mixed to obtain powder 5, 7-13% sticky yellow rice slurry of the mass of powder 4 is added to the powder 5, and then 0.1-0.3% water reducing agent of the mass of powder 4 is added, and the mixture is stirred evenly, and lightweight concrete is obtained by pouring, demoulding and curing.
2. The method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete according to claim 1, characterized in that: The carbonization treatment in step S6 is to carbonize for 3 to 6 hours in high temperature flue gas at 500 to 700°C.
3. The method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete according to claim 1, characterized in that: In the step S7, the S1 mixture, the S2 mixture, the S3 mixture, the purified sea sand in S4, and the powder 1 in S5 are mixed in a weight ratio of 5-10%: 5-8%: 50-60%: 20-30%: 3-5% to obtain a mixed material.
4. The method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete according to claim 1, characterized in that: The pressure of the pressing in step S7 is 15-25 MPa, and the pressed body is a cake with a thickness of 2-4 cm and a diameter of 5-8 cm.
5. The method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete according to claim 1, characterized in that: In step S8, the high temperature calcination is performed by heating from room temperature to 700°C at a heating rate of 5°C / min, and then keeping the temperature for 20 minutes; then heating from 700°C to 1100-1200°C at a heating rate of 10°C / min, and then keeping the temperature for 20-50 minutes.
6. The method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete according to claim 1, characterized in that: In step S8, the cooling is performed by blowing air for rapid cooling, and the cooling is performed to room temperature at a speed of 50°C / min.
7. The method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete according to claim 1, characterized in that: The calcination in step S10 is as follows: heating to 500° C. to 700° C. at a heating rate of 10 to 15° C. / min, and keeping the temperature for 3 to 5 hours.
8. The method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete according to claim 1, characterized in that: The soaking temperature of bagasse in step S12 is 45-55°C.
9. The method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete according to claim 1, characterized in that: During the cooking process in step S13, the mass concentration of the sticky yellow rice is maintained at 4-10%.
10. The method for preparing coal gasification slag-lithium slag-steel slag based lightweight concrete according to any one of claims 1 to 9, wherein in step S14, the powder 1 in S5, the low-carbon powder 2 in S9, and the powder 3 in S10 are mixed in a mass ratio of 5-10%:80-90%:5-10% to obtain powder 4; and the powder 4 is evenly mixed with the purified sea sand in S4 and the coarse aggregate in S11 in a mass ratio of 50-70%:15-30%:10-35% to obtain powder 5.
Citation Information
Cited By
Method for evaluating early cement hydration and product crystallization induced by two-component additive
CN119936083A
Methods for evaluating the early cement hydration and product crystallization induced by two-component additives
CN119936083B