Coking riser heat exchange equipment heat conduction mud and preparation method thereof
By using compositions such as potassium silicate solution, sodium silicate solution and sodium fluorosilicate with fine particle size in thermal conductivity, the problem of poor strain adhesion of thermal conductivity in high temperature, large temperature changes and strong corrosiveness is solved. The stability and self-cleaning function of thermally conductive mud are realized, and the heat exchange efficiency and service life of the coking riser are improved.
Patent Information
- Application Number
- CN202410862549.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-01
AI Technical Summary
The existing thermally conductive mud has poor strain adhesion in high temperature, large temperature changes and strong corrosive environments, which is prone to leakage and powdering, and lacks self-cleaning function, which affects the heat exchange efficiency and service life of the coke oven riser pipe.
Thermal mud formula with fine particle size, including potassium silicate solution, sodium silicate solution, dispersant BYK-190, Guangxi white mud, water-soluble fiber, scale graphite and artificial high power graphite, modified by homemade binder Enhance stability and strain force, and add sodium fluorosilicate to improve corrosion resistance.
In environments with high temperature, large temperature changes and strong corrosiveness, thermally conductive mud has good strain adhesion, is not easy to leak and powder, and has a self-cleaning function, which improves the heat exchange efficiency and service life of the coking rising pipe heat exchange equipment.
Smart Images

Figure CN118878338A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials and relates to a heat-conducting mud for coking riser heat exchange equipment and a preparation method thereof. Background Art
[0002] Coke oven gas, also known as raw gas or raw gas, is a high calorific value gas due to its high combustible components. Coke oven raw gas is a mixture, and its yield and composition vary depending on the quality of coking coal and the coking process. Raw gas carries corrosive factors such as oil vapor, water vapor, and benzene vapor. The main components are methane, carbon monoxide, water, hydrogen sulfide, and ammonia, which are highly corrosive. The mixed gas in the coke oven raw gas riser heat exchanger may produce tar at a temperature below 450°C. Tar is easy to adhere to the inner surface of the riser heat exchanger. Coal tar vapor condenses, causing condensation on the inner wall of the riser and blocking the riser channel; when the temperature is higher than 800°C, carbon will accumulate and graphite will grow; the coke oven riser heat exchanger must not leak water into the carbonization chamber, otherwise it will cause great damage to the coke oven body; this is the "three fears" often mentioned in the coking industry: fear of water leakage, fear of tar hanging, and fear of graphite growth. This causes the coke oven riser heat exchanger to be easily blocked, resulting in poor heat exchange effect, which seriously affects production. The coke oven riser heat exchanger plays a key role in the recovery of waste heat from sensible waste gas in the coke oven. The riser is insulated externally, improves the coking environment, and has good internal thermal conductivity. The inner tube is protected from tar and graphite. In order to increase the service life of the riser, the tube wall needs to be cooled by water. The current methods used are jacketed and spiral tube. Since there are many welds in the jacket type at the beginning, especially the annular seam at the lower part of the jacket due to the limitation of the structural form, the weld structure stress is large and it is easy to have uneven temperature fluctuations during use. Under the action of alternating stress, it is easy to tear, resulting in water leakage and inability to work normally. The spiral tube heat exchanger is designed with a higher working pressure and fewer welds, overcomes the welding defects of the jacket, and increases the service life. However, the heat conduction is not as balanced as the jacket. In order to make the coil type heat conduction effect balanced, it is necessary to add heat conduction medium and heat conduction mud in the coil gap.
[0003] The invention patent with the publication (announcement) number: CN105541356A discloses a high-temperature resistant thermal conductive mortar and its preparation method. The overall particle size is relatively coarse and the porosity is high. Due to the presence of air, the thermal conductivity is low. The core indicators of the thermal conductive mortar are high thermal conductivity, fast heat transfer, and high heat exchange efficiency on the equipment. It does not have the function of self-cleaning during use. Due to the coarse particle size, the tar generated by the fluctuation of the raw gas passing through the riser during use is easily adsorbed. Therefore, it does not have the self-cleaning function and cannot guarantee that there will be no tar hanging in the riser. The powder and liquid are packaged separately, which is inconvenient to use.
[0004] The patent application with publication (announcement) number: CN106085252A discloses a high-temperature resistant heat-insulating material, which adopts organic modified high-temperature resistant inorganic glue. It has great safety in use in complex high-temperature, large temperature difference and highly corrosive environments. Especially when it is resistant to temperature changes, the strength of the glue drops sharply, and local leakage, chemical reaction and powdering occur, resulting in the risk of maintenance of coking equipment and pipelines in long-term use, increasing the failure rate of equipment, affecting the waste heat recovery efficiency, and greatly restricting its use.
[0005] In summary, the existing thermal conductive mud has a coarse particle size, poor strain adhesion in high temperature, large temperature change and highly corrosive environments, is resistant to temperature changes, is easy to leak and powder, and does not have a self-cleaning function. Summary of the invention
[0006] The purpose of the present invention is to provide a thermal conductive mud for coking riser heat exchange equipment and a preparation method thereof, so as to solve the technical problems that the existing thermal conductive mud has a coarse particle size, poor strain adhesion in a high temperature, large temperature change and highly corrosive environment, and is easy to leak and pulverize due to temperature changes. The thermal conductive mud of the present invention has a finer particle size and has better strain adhesion in a high temperature, large temperature change and highly corrosive environment. The thermal conductive mud is not easy to leak and pulverize, has good stability, and has a self-cleaning function.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The invention discloses a heat-conducting mud for a coking riser heat exchange device, comprising a composition consisting of a potassium silicate solution, a sodium silicate solution, a dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a quantitative ratio of (25-27): (25-27): (0.3-0.4): (1.5-2): (0.8-1): (30-32): (8-10): (3-5).
[0009] Furthermore, sodium fluorosilicate is added to the composition, and the sodium fluorosilicate accounts for 2% to 5% of the total mass of the composition.
[0010] Furthermore, the purity of sodium fluorosilicate is greater than or equal to 99%
[0011] Furthermore, the modulus of the potassium silicate solution is 2.8-3.0, and the effective content is 40-42%, and the modulus of the sodium silicate solution is 2.8-3.0, and the effective content is 42-45%.
[0012] Furthermore, the Guangxi white mud is 200-300 mesh, the aluminum oxide content is greater than or equal to 34%, and the iron oxide content is less than 1.5%.
[0013] Furthermore, the water-soluble fiber is AX water-soluble fiber.
[0014] Further, the flake graphite #100 is 100 mesh, with a purity of more than 99%, and the flake graphite #50 is 50 mesh, with a purity of more than 99%.
[0015] Furthermore, the specification of artificial high-power graphite is 1mm and the purity is more than 95%.
[0016] Based on the above heat-conducting mud, the present invention also discloses a method for preparing heat-conducting mud for coking riser heat exchange equipment, comprising the following steps:
[0017] Weigh potassium silicate solution, sodium silicate solution, dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a weight ratio of (25-27): (25-27): (0.3-0.4): (1.5-2): (0.8-1): (30-32): (8-10): (3-5);
[0018] The potassium silicate solution, the sodium silicate solution and the dispersant BYK-190 are mixed and stirred for 20 to 40 minutes to obtain a mixture A;
[0019] Add Guangxi white mud and water-soluble fiber to mixture A, mix and stir for 10 to 30 minutes to obtain mixture B;
[0020] Flake graphite #100, flake graphite #50 and artificial high-power graphite were added to mixture B, and the mixture was kneaded at a rotation speed of 300 to 400 rpm for 20 minutes, and then kneaded at a rotation speed of 150 rpm until it was in a paste state to obtain a composition.
[0021] Furthermore, sodium fluorosilicate is added to the composition and mixed evenly when used, and the sodium fluorosilicate accounts for 2% to 5% of the total mass of the composition.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The thermal conductive mud of the present invention comprises a composition consisting of potassium silicate solution, sodium silicate solution, dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a quantitative ratio of (25-27): (25-27): (0.3-0.4): (1.5-2): (0.8-1): (30-32): (8-10): (3-5). The thermal conductive mud of the present invention has a finer particle size than the existing thermal conductive mud; the present invention modifies the binder by using a homemade adhesive thickener to enhance the stability of the high temperature resistant thermal conductive mud and improve the high and low temperature strain resistance. It has good strain adhesion in high temperature, large temperature change and highly corrosive environments. The thermal conductive mud is not easy to leak and powderize, and has good stability; by adjusting the formula to improve the high temperature resistance and corrosion resistance of the thermal insulation layer, it can meet various complex working conditions inside the riser heat exchange equipment, prevent tar from hanging, and fully have the function of self-cleaning. The heat exchange efficiency of the coking riser heat exchange equipment is improved.
[0024] 2. The method of the present invention is to mix potassium silicate solution, sodium silicate solution and dispersant BYK-190 for 20 to 40 minutes to obtain mixture A; Guangxi white mud and water-soluble fiber are added to mixture A, and mixed and stirred for 10 to 30 minutes to obtain mixture B; flake graphite #100, flake graphite #50 and artificial high-power graphite are added to mixture B, and kneaded at a speed of 300 to 400 rpm for 20 minutes, and then kneaded at a speed of 150 rpm to a paste to obtain a composition. The present invention modifies the binder by using a homemade binder thickener to enhance the stability of the high-temperature resistant thermal conductive mud while improving the high and low temperature strain resistance; by adjusting the formula to improve the high temperature resistance and corrosion resistance of the thermal insulation layer, it can meet a variety of complex working conditions inside the riser heat exchange equipment, prevent tar from hanging, and fully have the function of self-cleaning. Improve the heat exchange efficiency of the coking riser heat exchange equipment. Compared with the existing thermal conductive mud with finer particle size, it has better strain adhesion in high temperature, large temperature change and highly corrosive environment. The thermal conductive mud is not easy to leak or powderize and has good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The figure is a flow chart of the method of the present invention. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0027] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0028] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0029] The invention discloses a thermal conductive mud for a coking riser heat exchanger, comprising a composition consisting of a potassium silicate solution, a sodium silicate solution, a dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a quantitative ratio of (25-27): (25-27): (0.3-0.4): (1.5-2): (0.8-1): (30-32): (8-10): (3-5). Compared with the existing thermal conductive mud, the thermal conductive mud of the invention has a finer particle size, has better strain adhesion in an environment with high temperature, large temperature change and strong corrosiveness, is not easy to leak and pulverize, and has good stability. The invention modifies the binder by making a tackifier of the binder, thereby enhancing the stability of the high temperature resistant heat conductive mud and improving the high and low temperature strain resistance; by adjusting the formula, the high temperature resistance and corrosion resistance of the thermal insulation layer are improved, and various complex working conditions inside the riser heat exchange equipment can be met. The dispersant BYK-190 used in the invention has high purity and ultrafine powder, as well as a reasonable formula structure and preparation process, which can prevent the heat conductive mud from hanging tar and fully have the function of self-cleaning. The heat exchange efficiency of the coking riser heat exchange equipment is improved.
[0030] Embodiment 1:
[0031] The present embodiment discloses a thermal conductive mud for coking riser heat exchange equipment, including a composition consisting of a potassium silicate solution, a sodium silicate solution, a dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a quantitative ratio of 25:25:0.3:1.5:0.8:30:8:3.
[0032] Preferably, sodium fluorosilicate is added to the composition, and the sodium fluorosilicate accounts for 2% to 5% of the total mass of the composition.
[0033] Preferably, the purity of sodium fluorosilicate is greater than or equal to 99%
[0034] Preferably, the modulus of the potassium silicate solution is 2.8 and the effective content is 40%, and the modulus of the sodium silicate solution is 2.8 and the effective content is 42%.
[0035] Preferably, Guangxi white mud is 200 mesh, the aluminum oxide content is greater than or equal to 34%, and the iron oxide content is less than 1.5%.
[0036] Preferably, the water-soluble fiber is AX water-soluble fiber.
[0037] Preferably, the flake graphite #100 is 100 mesh and has a purity of more than 99%, and the flake graphite #50 is 50 mesh and has a purity of more than 99%.
[0038] Preferably, the specification of artificial high-power graphite is 1 mm and the purity is above 95%.
[0039] The thermal conductive mud obtained in this embodiment has been used in the field for 2 months. There is no leakage of thermal conductive mud due to heat softening, no powdering due to high-temperature chemical reaction, no softening and deterioration due to high temperature, no change in hardness, strength or color at room temperature. Compared with the existing thermal conductive mud, the thermal conductive mud has stronger thermal conductivity, and its high temperature resistance and high and low temperature fastness are also significantly improved. The service life of the riser is increased, and the waste heat recovery is better.
[0040] Embodiment 2:
[0041] The invention discloses a thermal conductive mud for a coking riser heat exchange device, comprising a composition consisting of a potassium silicate solution, a sodium silicate solution, a dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a quantitative ratio of 26:26:0.35:1.75:0.9:31:9:4.
[0042] Preferably, sodium fluorosilicate is added to the composition, and the sodium fluorosilicate accounts for 3.5% of the total mass of the composition.
[0043] Preferably, the purity of sodium fluorosilicate is greater than or equal to 99%
[0044] Preferably, the modulus of the potassium silicate solution is 2.9 and the effective content is 41%, and the modulus of the sodium silicate solution is 2.9 and the effective content is 43.5%.
[0045] Preferably, Guangxi white mud is 250 mesh, the aluminum oxide content is greater than or equal to 34%, and the iron oxide content is less than 1.5%.
[0046] Preferably, the water-soluble fiber is AX water-soluble fiber.
[0047] Preferably, the flake graphite #100 is 100 mesh and has a purity of more than 99%, and the flake graphite #50 is 50 mesh and has a purity of more than 99%.
[0048] Preferably, the specification of artificial high-power graphite is 1 mm and the purity is above 95%.
[0049] The thermal conductive mud obtained in this embodiment has been used in the field for 2 months. There is no leakage of thermal conductive mud due to heat softening, no powdering due to high-temperature chemical reaction, no softening and deterioration due to high temperature, no change in hardness, strength or color at room temperature. Compared with the existing thermal conductive mud, the thermal conductive mud has stronger thermal conductivity, and its high temperature resistance and high and low temperature fastness are also significantly improved. The service life of the riser is increased, and the waste heat recovery is better.
[0050] Embodiment three:
[0051] The invention discloses a heat-conducting mud for a coking riser heat exchange device, comprising a composition consisting of a potassium silicate solution, a sodium silicate solution, a dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a quantitative ratio of 27:27:0.4:2:1:32:10:5.
[0052] Preferably, sodium fluorosilicate is added to the composition, and the sodium fluorosilicate accounts for 5% of the total mass of the composition.
[0053] Preferably, the purity of sodium fluorosilicate is greater than or equal to 99%
[0054] Preferably, the modulus of the potassium silicate solution is 3.0 and the effective content is 42%, and the modulus of the sodium silicate solution is 3.0 and the effective content is 45%.
[0055] Preferably, Guangxi white mud is 300 mesh, the aluminum oxide content is greater than or equal to 34%, and the iron oxide content is less than 1.5%.
[0056] Preferably, the water-soluble fiber is AX water-soluble fiber.
[0057] Preferably, the flake graphite #100 is 100 mesh and has a purity of more than 99%, and the flake graphite #50 is 50 mesh and has a purity of more than 99%.
[0058] Preferably, the specification of artificial high-power graphite is 1 mm and the purity is above 95%.
[0059] The thermal conductive mud obtained in this embodiment has been used in the field for 2 months. There is no leakage of thermal conductive mud due to heat softening, no powdering due to high-temperature chemical reaction, no softening and deterioration due to high temperature, no change in hardness, strength or color at room temperature. Compared with the existing thermal conductive mud, the thermal conductive mud has stronger thermal conductivity, and its high temperature resistance and high and low temperature fastness are also significantly improved. The service life of the riser is increased, and the waste heat recovery is better.
[0060] Embodiment 4:
[0061] This embodiment discloses a thermal conductive mud for a coking riser heat exchanger. To overcome the shortcomings of the thermal conductive mud used in the conventional industry, such as poor high and low temperature strain adhesion and weak corrosion resistance, the formula of the thermal conductive mud in the coking riser heat exchanger is as follows:
[0062] Taking the total mass of 200KG as an example, the formula includes the following components:
[0063]
[0064] Formula raw material procurement requirements:
[0065] 01 Material code: BK potassium silicate solution, modulus 2.8-3.0, effective content 40-42%;
[0066] 02 Material code: BN sodium silicate solution, modulus 2.8-3.0, effective content 42-45%;
[0067] 03Material code: BY dispersant BYK-190, model BYK-190;
[0068] 04 Material code: AN Guangxi white mud, 200 mesh ~ 300 mesh, aluminum oxide ≥ 34%, iron oxide < 1.5%;
[0069] 05 Material code: AX water-soluble fiber, soluble in water at 80℃;
[0070] 06Material code: A10 flake graphite #100, 100 mesh, purity above 99%;
[0071] 07Material code: A5 flake graphite #50, 50 mesh, purity above 99%;
[0072] 08Material code: A1 artificial high power graphite, 1mm, purity above 95%;
[0073] 09 Material code: AF sodium fluorosilicate, purity ≥99%;
[0074] Based on the above-mentioned thermal conductive mud for coking riser heat exchange equipment, the present invention discloses a method for preparing thermal conductive mud for coking riser heat exchange equipment, comprising the following steps:
[0075] S1. Weigh potassium silicate solution, sodium silicate solution, dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a weighing ratio of (25-27): (25-27): (0.3-0.4): (1.5-2): (0.8-1): (30-32): (8-10): (3-5);
[0076] S2. The potassium silicate solution, the sodium silicate solution and the dispersant BYK-190 are mixed and stirred for 20 to 40 minutes to obtain a mixture A;
[0077] S3. Add Guangxi white mud and water-soluble fiber to mixture A, mix and stir for 10 to 30 minutes to obtain mixture B;
[0078] S4. Add flake graphite #100, flake graphite #50 and artificial high-power graphite to mixture B, knead at a speed of 300 to 400 rpm for 20 minutes, and then knead at a speed of 150 rpm to obtain a paste-like composition.
[0079] Preferably, sodium fluorosilicate is added to the composition and mixed evenly when used, and the sodium fluorosilicate accounts for 2% to 5% of the total mass of the composition.
[0080] The thermal conductive mud prepared by the method of the present invention has a finer particle size than the existing thermal conductive mud, has better strain adhesion in high temperature, large temperature change and highly corrosive environment, is not easy to leak and powder, and has good stability. The present invention modifies the binder by using a homemade binder thickener to enhance the stability of the high temperature resistant thermal conductive mud while improving the high and low temperature strain resistance; by adjusting the formula to improve the high temperature resistance and corrosion resistance of the thermal insulation layer, it can meet the various complex working conditions inside the riser heat exchange equipment, prevent tar from hanging, and fully have the function of self-cleaning. Improve the heat exchange efficiency of the coking riser heat exchange equipment.
[0081] Embodiment five:
[0082] The present embodiment provides a method for preparing thermal conductive mud for a coking riser heat exchange equipment, comprising the following steps:
[0083] S1. Weigh potassium silicate solution, sodium silicate solution, dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a ratio of 25:25:0.3:1.5:0.8:30:8:3;
[0084] S2. The potassium silicate solution, the sodium silicate solution and the dispersant BYK-190 were added to the kneader, stirring was started, the speed was controlled at 200 rpm, and the mixture was stirred for 20 minutes to obtain a mixture A;
[0085] S3. Add Guangxi white mud and water-soluble fiber to the mixture A, maintain the stirring speed at 200 rpm, and mix and stir for 10 minutes to obtain a mixture B;
[0086] S4. Add flake graphite #100, flake graphite #50 and artificial high-power graphite to mixture B, start the dust removal equipment at the same time, knead at a speed of 300 rpm for 20 minutes, and then knead at a speed of 150 rpm to obtain a paste-like composition.
[0087] Preferably, sodium fluorosilicate is added to the composition and mixed evenly when used, and the sodium fluorosilicate accounts for 2% of the total mass of the composition.
[0088] Embodiment six:
[0089] The present embodiment provides a method for preparing thermal conductive mud for a coking riser heat exchange equipment, comprising the following steps:
[0090] S1. Weigh potassium silicate solution, sodium silicate solution, dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a ratio of 26:26:0.35:1.75:0.9:31:9:4;
[0091] S2. The potassium silicate solution, the sodium silicate solution and the dispersant BYK-190 were added to the kneader, stirring was started, the speed was controlled at 200 rpm, and the mixture was stirred for 30 minutes to obtain a mixture A;
[0092] S3. Add Guangxi white mud and water-soluble fiber to the mixture A, maintain the stirring speed at 200 rpm, and mix and stir for 20 minutes to obtain a mixture B;
[0093] S4. Add flake graphite #100, flake graphite #50 and artificial high-power graphite to mixture B, start the dust removal equipment at the same time, knead at a speed of 350 rpm for 20 minutes, and then knead at a speed of 150 rpm to obtain a paste-like composition.
[0094] Preferably, sodium fluorosilicate is added to the composition and mixed evenly when used, and the sodium fluorosilicate accounts for 3.5% of the total mass of the composition.
[0095] Embodiment seven:
[0096] The present embodiment provides a method for preparing thermal conductive mud for a coking riser heat exchange equipment, comprising the following steps:
[0097] S1. Weigh potassium silicate solution, sodium silicate solution, dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a ratio of 27:27:0.4:2:1:32:10:5;
[0098] S2. The potassium silicate solution, the sodium silicate solution and the dispersant BYK-190 were added to the kneader, stirring was started, the speed was controlled at 200 rpm, and the mixture was stirred for 40 minutes to obtain a mixture A;
[0099] S3. Add Guangxi white mud and water-soluble fiber to the mixture A, maintain the stirring speed at 200 rpm, and mix and stir for 30 minutes to obtain a mixture B;
[0100] S4. Add flake graphite #100, flake graphite #50 and artificial high-power graphite to mixture B, start the dust removal equipment at the same time, knead at a speed of 400 rpm for 20 minutes, and then knead at a speed of 150 rpm to obtain a paste-like composition.
[0101] Preferably, sodium fluorosilicate is added to the composition and mixed evenly when used, and the sodium fluorosilicate accounts for 5% of the total mass of the composition.
[0102] Embodiment eight:
[0103] This embodiment provides a method for preparing thermal conductive mud for coking riser heat exchange equipment, comprising the following steps:
[0104] S1. Add the weighed materials BK and BN into the kneader, start stirring, control the speed at 200 rpm, add the pre-weighed material BY, and stir for 20-40 minutes after adding.
[0105] S2. Add the pre-weighed materials AN and AX into the feeder, keep the stirring speed at 200 rpm, and continue for 10-30 minutes after the addition is completed.
[0106] S3. Slowly add pre-weighed materials A10, A5, and A1 to the kneader through the feeder, and start the dust removal equipment at the same time. Add them in no order and increase the speed to 300-400 rpm. After kneading for 20 minutes, knead at a low speed of 150 rpm. Keep the site free of dust to avoid material loss. After 30-40 minutes of adding materials A10, A5, and A1, knead for 30-50 minutes until they are evenly kneaded into a paste. The kneading roll of the kneading machine rotates clockwise and counterclockwise for 10 minutes at intervals. The material can be discharged only after the sampling inspection is qualified.
[0107] S4. Discharging: Keep the kneading machine meshing roller rotating clockwise at a speed of 200 rpm, and the discharging roller rotating counterclockwise at 500-600 rpm. Pack the mixture into a packaging barrel lined with a sealing bag and seal it for storage.
[0108] Embodiment nine:
[0109] In this embodiment, the above-mentioned thermal conductive mud of the coking riser heat exchange equipment is used. The coking riser of the first coking plant uses the thermal conductive mud produced according to the above-mentioned proportion. One riser is made to conduct experiments in the coking plant to verify the effect:
[0110] Rising pipe field working condition experiment: Install the experimental product into working state:
[0111] After 2 months of field use
[0112] There is no leakage of thermal conductive mud due to softening due to heat, no powdering due to high-temperature chemical reaction, no softening and deterioration due to high temperature, and the thermal conductive mud does not change in hardness, strength, or color at room temperature.
[0113] Existing problems: The storage problem of the produced thermal conductive paste needs to be improved to improve the sealing performance, and the sealing performance of the thermal conductive paste should be improved during mass production.
[0114] Embodiment 10:
[0115] In this embodiment, the above-mentioned heat transfer mud of the coking riser heat exchange equipment is used, and the second coking plant is used for the new riser condition:
[0116] The formula of the above embodiment is adjusted, and the basic properties of the adjusted thermal conductive mud and the existing thermal conductive mud of the comparative example are shown in Table 1:
[0117] Table 1. Comparison of basic properties of thermal conductive pastes of the above embodiments and comparative examples:
[0118]
[0119] According to the design and use requirements of the coke oven coking riser heat exchange equipment, it is concluded based on the test of this patent that the thermal conductivity of the thermal conductive mud in the embodiment is significantly higher than the mainstream market formula of the comparison example, indicating that the thermal conductivity of the newly developed thermal conductive mud is stronger; it is significantly higher than the comparison example, and the high temperature resistance and high and low temperature fastness are also significantly improved, indicating that the high temperature resistance and high and low temperature resistance of the newly developed thermal conductive mud are significantly better than conventional products on the market; through use in the coking plant, the service life of the riser is increased, and the waste heat recovery is better. The embodiment of this patent is significantly better than the products used in the market, indicating that it has stronger practical performance.
[0120] In summary, compared with the prior art, the present invention has the following technical effects:
[0121] In view of the low thermal conductivity of traditional thermal conductive mud, the high temperature is easy to produce deterioration chemical reaction, and high temperature leakage and pulverization, resulting in uneven temperature of the inner tube of the riser, in order to overcome the high temperature insulation aluminum silicate wool insulation and thermal insulation felt commonly used in the existing traditional industrial thermal insulation industry equipment to make the thermal conductive mud balanced in thermal conductivity and resistant to high and low temperature strain, the present invention modifies the binder with a homemade binder thickener, thereby enhancing the stability of the high temperature resistant thermal conductive mud and improving the resistance to high and low temperature strain; by adjusting the formula, the high temperature resistance and corrosion resistance of the thermal insulation layer are improved, which can meet the various complex working conditions inside the riser heat exchange equipment, prevent tar from hanging, and have a complete self-cleaning function, thereby improving the heat exchange efficiency of the coking riser heat exchange equipment, reducing the risk of maintenance, reducing the cost of maintenance, and improving the production efficiency. It is cost-effective and can meet the large-scale promotion of the market.
[0122] Thermal mud is a medium filled between spiral tubes to balance the heat conduction of the inner tube of the riser, ensuring that the inner tube of the riser has a relatively stable temperature range. It improves the preheating recovery efficiency of the riser, avoids low gas production due to low temperature, shortened life of the riser due to high temperature, and even leads to shutdown. Therefore, thermal mud plays a role of balanced heat conduction between the coils of the riser. The thermal mud has a good thermal conductivity effect, which can increase the waste heat recovery gas production of the riser. At the same time, the temperature of the inner tube of the riser is balanced and not easy to burn, which can increase the service life of the riser. If the thermal mud is not effective, the result will be the opposite.
[0123] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A thermal conductive mud for coking riser heat exchange equipment, characterized in that: The invention discloses a composition comprising potassium silicate solution, sodium silicate solution, dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a quantitative ratio of (25-27): (25-27): (0.3-0.4): (1.5-2): (0.8-1): (30-32): (8-10): (3-5).
2. The thermal conductive mud for coking riser heat exchange equipment according to claim 1, characterized in that: Sodium fluorosilicate is added into the composition, and the sodium fluorosilicate accounts for 2% to 5% of the total mass of the composition.
3. The thermal conductive mud for coking riser heat exchange equipment according to claim 2, characterized in that: The purity of the sodium fluorosilicate is greater than or equal to 99%.
4. The thermal conductive mud for coking riser heat exchange equipment according to claim 1, characterized in that: The modulus of the potassium silicate solution is 2.8-3.0, and the effective content is 40-42%. The modulus of the sodium silicate solution is 2.8-3.0, and the effective content is 42-45%.
5. The thermal conductive mud for coking riser heat exchange equipment according to claim 1, characterized in that: The Guangxi white mud has a mesh size of 200 to 300, an aluminum oxide content of 34% or more, and a iron oxide content of less than 1.5%.
6. The thermal conductive mud for coking riser heat exchange equipment according to claim 1, characterized in that: The water-soluble fiber is AX water-soluble fiber.
7. The thermal conductive mud for coking riser heat exchange equipment according to claim 1, characterized in that: The flake graphite #100 has a mesh size of 100 and a purity of more than 99%, and the flake graphite #50 has a mesh size of 50 and a purity of more than 99%.
8. The thermal conductive mud for coking riser heat exchange equipment according to claim 1, characterized in that: The specification of the artificial high-power graphite is 1 mm, and the purity is above 95%.
9. A method for preparing thermal conductive mud for coking riser heat exchange equipment according to any one of claims 1 to 8, characterized in that: The following steps are involved: Weigh potassium silicate solution, sodium silicate solution, dispersant BYK-190, Guangxi white mud, water-soluble fiber, flake graphite #100, flake graphite #50 and artificial high-power graphite in a weight ratio of (25-27): (25-27): (0.3-0.4): (1.5-2): (0.8-1): (30-32): (8-10): (3-5); The potassium silicate solution, the sodium silicate solution and the dispersant BYK-190 are mixed and stirred for 20 to 40 minutes to obtain a mixture A; Add Guangxi white mud and water-soluble fiber to mixture A, mix and stir for 10 to 30 minutes to obtain mixture B; Flake graphite #100, flake graphite #50 and artificial high-power graphite were added to mixture B, and the mixture was kneaded at a rotation speed of 300 to 400 rpm for 20 minutes, and then kneaded at a rotation speed of 150 rpm until it was in a paste state to obtain a composition.
10. The method for preparing thermal conductive mud for coking riser heat exchange equipment according to claim 9, characterized in that: The composition is added with sodium fluorosilicate and mixed evenly when in use, and the sodium fluorosilicate accounts for 2% to 5% of the total mass of the composition.
Citation Information
Patent Citations
High-temperature-resistant cement and preparation method for same
CN105541356A
Heat transfer cement, preparation method and application thereof
CN106085252A
Heat-resisting compact inorganic hole sealing agent coating
CN103172344A
Environment-friendly iron runner castable and preparation method thereof
CN116143529A
Heat conduction material as well as preparation method and application thereof
CN117550871A