High molecular weight thermoplastic phenolic resin with narrow molecular weight distribution and preparation method thereof

A high molecular weight thermoplastic phenolic resin with a narrow molecular weight distribution was successfully prepared by polymerization of dihydroxydiphenylmethane and formaldehyde and xylene extraction process, which solved the problem of wide molecular weight distribution in the prior art and improved the char yield of the resin and the performance of the composite material.

CN118878764AActive Publication Date: 2024-11-01XI AN JIAOTONG UNIV

Patent Information

Application Number
CN202410993802.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-01
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing technologies make it difficult to simultaneously achieve high molecular weight and narrow molecular weight distribution thermoplastic phenolic resins, resulting in low polydispersity and char formation of the resin, which affects the performance of composite materials.

Method used

By using the polymerization reaction of dihydroxydiphenylmethane and formaldehyde, combined with xylene extraction, and by controlling the reaction conditions and purification process, high molecular weight thermoplastic phenolic resin with narrow molecular weight distribution can be prepared, thereby reducing polydispersity.

Benefits of technology

The prepared thermoplastic phenolic resin has a weight-average molecular weight of 2600 g/mol, a molecular weight distribution index as low as 1.79, a char formation rate of 63.0%, and an interlaminar shear strength of 55 MPa.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878764A_ABST
    Figure CN118878764A_ABST
Patent Text Reader

Abstract

The invention discloses a high-molecular-weight thermoplastic phenolic resin with narrow molecular weight distribution and a preparation method thereof, and the preparation method of the resin comprises two steps: a polymerization process and a xylene extraction process. According to the invention, dihydroxydiphenylmethane is taken as an initial raw material, so that the resin obtained by polymerization has narrower molecular weight distribution than that of traditional phenolic resin; furthermore, part or most of low-molecular-weight components in the resin are removed through xylene extraction, so that the molecular weight distribution of the resin is further narrowed while the average molecular weight of the resin is improved, and the aim of remarkably improving the carbon yield of the resin is achieved; the weight-average molecular weight of the prepared thermoplastic phenolic resin reaches 2600g / mol or above, and meanwhile, the molecular weight distribution index is as low as 1.79; as the molecular weight is increased and the molecular weight distribution is narrowed, the char yield of the resin is increased; after the resin is cured by hexamethylenetetramine, the highest char forming rate can reach 63.0%, and the interlaminar shear strength of a carbon fiber reinforced composite material reaches 55MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials and relates to resins, in particular to a high molecular weight thermoplastic phenolic resin with a narrow molecular weight distribution and a preparation method thereof. Background Art

[0002] In the development process of thermoplastic phenolic resin, people have been paying attention to the influence of thermoplastic phenolic resin and its molecular weight on the performance of the resin, especially in the field of phenolic resin-based ablation-resistant composite materials, the molecular weight of thermoplastic phenolic resin is an important factor that seriously affects the charring rate of the resin. Studies have shown that thermoplastic phenolic resin with higher molecular weight has fewer end groups, and can achieve a higher degree of cross-linking and fewer end groups at a lower curing agent dosage, reducing the probability of forming volatile organic compounds (such as phenol, cresol, etc.) when the cured phenolic resin undergoes thermal decomposition, thereby increasing the thermal decomposition temperature and charring rate of the resin.

[0003] With the development of science and technology and the expansion of the application field of phenolic resin, people realize that the molecular weight distribution of phenolic resin is also a major factor affecting the performance of phenolic resin. It is generally believed that (2000, Zhao Tong et al., CN1124299C) relative to ordinary phenolic resin, phenolic resin with narrow molecular weight distribution has lower melt viscosity and more uniform curing behavior, and the heat resistance and toughness of the product are better. Patent (2023, CN 117164789 A's point of view) points out that in the field of rubber application, the molecular weight distribution of conventional phenolic resin is relatively wide, resulting in poor compatibility with rubber, resulting in poor mechanical properties and processing properties of the rubber.

[0004] However, in the traditional process of synthesizing phenolic resins using phenol and formaldehyde as raw materials, based on the characteristics of its polymerization reaction, the molecular weight of thermoplastic phenolic resins gradually grows up, that is, phenol is converted into dimer, dimer is converted into trimer, ..., and finally forms a product with a higher molecular weight. However, since the substituted phenol ring is easier to further react with formaldehyde than the phenol raw material, when the raw material formaldehyde is consumed, in addition to the resin molecules with a higher molecular weight, a large amount of phenol will remain in the system. Due to this molecular weight distribution characteristic, the molecular weight distribution of phenolic resins is wider, especially with the formation of higher molecular weight molecules, although the average molecular weight of the resin has increased, the molecular weight distribution of the resin is also wider.

[0005] The molecular weight distribution of phenolic resin is expressed as the weight average molecular weight of the resin. and number average molecular weight The ratio of is called polydispersity index (PDI):

[0006] Based on the strong polarity and low molecular weight of phenol, it can be removed by water washing or distillation in industry to prepare thermoplastic phenolic resin with very low free phenol content (less than 1%). With the removal of phenol, the average molecular weight of phenolic resin will increase and PDI will decrease. However, phenolic resin inevitably contains a large number of dimers. In commercially available thermoplastic phenolic resins, dimers are often the highest content fraction relative to the polymerization products of each degree of polymerization above trimer, and the content can be as high as 10%. Based on this characteristic of the polymerization reaction of phenol and formaldehyde, in order to obtain a resin with a higher average molecular weight, a certain amount of high molecular weight fraction must be present, resulting in a wider molecular weight distribution of the resin, that is, a larger PDI. For example, the phenolic resin with a weight average molecular weight of 6600g / mol and a number average molecular weight of 1500g / mol sold on the market has a PDI of 4.36; the phenolic resin with a weight average molecular weight of 2350g / mol and a number average molecular weight of 1060g / mol has a PDI of 2.22.

[0007] In other words, if phenol is used as a raw material to synthesize a thermoplastic phenolic resin, its strong molecular weight polydispersity is difficult to avoid. Although there are reports of thermoplastic phenolic resins with narrow molecular weight distribution, the average molecular weight of these resins is mostly not high, that is, they are lower PDIs achieved at lower average molecular weights. For example, CN 117164789 A (2023) discloses a method for preparing a narrow molecular weight distribution phenolic resin, wherein the PDI of the resin is less than 1.9, but its weight average molecular weight is between 1700 and 2300 g / mol. It can be seen that it is not easy to prepare a thermoplastic phenolic resin with both high molecular weight and narrow molecular weight distribution. Summary of the invention

[0008] In view of the shortcomings of the prior art, the object of the present invention is to provide a high molecular weight thermoplastic phenolic resin with a narrow molecular weight distribution and a preparation method thereof.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] A method for preparing a high molecular weight thermoplastic phenolic resin with a narrow molecular weight distribution comprises the following steps:

[0011] Step 1, adding dihydroxydiphenylmethane, formaldehyde aqueous solution, organic solvent and oxalic acid into a reaction kettle; wherein the molar ratio of dihydroxydiphenylmethane to formaldehyde is 1:(0.8-1.2); the mass ratio of dihydroxydiphenylmethane to organic solvent is 100:(40-100); the mass ratio of dihydroxydiphenylmethane to oxalic acid is 100:(0.5-5); the organic solvent includes an organic compound that is miscible with water and has good solubility in dihydroxydiphenylmethane;

[0012] Step 2: After purging with nitrogen, close the reactor, heat it to 80-100°C, control the pressure in the reactor to 0.105-0.110 MPa, and keep the reaction at this temperature for 1-4 hours; heat it to 100-120°C, keep the reaction at this temperature for 1-4 hours, and control the pressure in the reactor to be no more than 0.2 MPa;

[0013] Step 3: Pass nitrogen protection, raise the temperature to 120-140°C, perform atmospheric distillation to remove most of the water and organic solvents; then perform reduced pressure distillation at -0.09-0.08MPa, and heat the kettle to raise the temperature to 160-165°C, and maintain for 0.2-1.0h; finally, restore the normal pressure, and cool down to 130-140°C under nitrogen protection;

[0014] Step 4: extracting the product of step 3 with xylene to obtain a high molecular weight thermoplastic phenolic resin with a narrow molecular weight distribution.

[0015] The present invention also has the following technical features:

[0016] Preferably, the mass percentage concentration of the formaldehyde aqueous solution in step 1 is 35.0-38.0%.

[0017] Preferably, the organic solvent includes any one of ethanol, methanol, acetone and tetrahydrofuran.

[0018] Preferably, the xylene described in step 4 includes any one of o-xylene, p-xylene or m-xylene, or a mixture of any proportions of the two or more thereof.

[0019] Preferably, the method of extracting the product of step 3 using xylene in step 4 comprises:

[0020] S1: Add xylene to the reaction kettle, pass nitrogen, stir at a speed of 20-100 rpm, heat to reflux for 10-30 minutes, stop stirring, let stand for 20-40 minutes, and after the xylene and resin in the kettle are separated, suck out the upper layer of xylene; wherein the mass ratio of xylene to dihydroxydiphenylmethane is 100:(50-200);

[0021] S2 repeats the operation of S1 2 to 6 times, and at the same time determines the molecular weight, distribution and composition of the resin by gel permeation chromatography (GPC). When the molecular weight of the resin reaches the requirement, the extraction process is completed;

[0022] S3 is distilled under reduced pressure at 140°C to remove xylene, and discharged at 135-145°C under normal pressure to obtain a high molecular weight thermoplastic phenolic resin with a narrow molecular weight distribution.

[0023] The present invention also protects a high molecular weight thermoplastic phenolic resin with narrow molecular weight distribution prepared by the method as described above.

[0024] Compared with the prior art, the present invention has the following technical effects:

[0025] The invention prepares a high molecular weight thermoplastic phenolic resin with narrow molecular weight distribution in a reactor through polymerization reaction and refining extraction. The traditional method using phenol as a raw material is abandoned. Instead, dihydroxydiphenylmethane (BPM) is used as a raw material. The thermoplastic phenolic resin is synthesized through polymerization reaction between BPM and formaldehyde, thereby reducing the polydispersity of the molecular weight of the phenolic resin and making its molecular weight distribution narrower. Furthermore, through the refining process of xylene extraction, the stronger solubility of xylene in the low molecular weight fraction in the phenolic resin can partially or mostly remove the low molecular weight fraction, such as part of dimers, trimers and tetramers, thereby reducing the polydispersity of the resin molecular weight while increasing the average molecular weight of the resin, that is, reducing the PDI. The xylene extraction process completely overcomes the limitation of the traditional method for synthesizing high molecular weight phenolic resin.

[0026] The thermoplastic phenolic resin prepared by the present invention has a weight average molecular weight of up to 2600 g / mol and a minimum molecular weight distribution index of 1.79; further, as the molecular weight increases and the molecular weight distribution becomes narrower, the charring rate of the resin increases; after the resin is cured by hexamethylenetetramine, the charring rate can reach up to 63.0%, and the interlaminar shear strength of the carbon fiber reinforced composite material reaches 55 MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 1 is the GPC curve of the thermoplastic phenolic resin obtained in Example 1 and Comparative Example 1;

[0028] Figure 2 It is the GPC curve of the thermoplastic phenolic resin obtained in Comparative Example 2, Example 2, Example 3 and Example 4. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical effect and technical solution of the embodiment of the present invention clearer, the technical solution in the embodiment of the present invention is clearly and completely described below in conjunction with the drawings in the embodiment of the present invention; it is obvious that the embodiment described here is a part of the embodiment of the present invention. Based on the embodiment disclosed in the present invention, other embodiments obtained by ordinary technicians in this field without making creative work should all fall within the scope of protection of the present invention.

[0030] In the following embodiments, the dihydroxydiphenylmethane used, referred to as BPM, commonly known as bisphenol F, methylene bisphenol, bis-(hydroxyphenyl) methane, is provided by Shanghai Licas Industrial Co., Ltd., with a purity of 92.5% and a melting point of 113.1°C.

[0031] The purity of the adopted organic solvent and oxalic acid is greater than 99%.

[0032] The xylene used includes any one of o-xylene, p-xylene or m-xylene or a mixture of any proportions of the two or more of the o-xylene.

[0033] The molecular weight and composition of the resin were determined using a 1260 gel permeation chromatograph (GPC) from Agilent, USA. Plgel and Plgel Used in series, the column temperature was 40°C, chromatographic grade tetrahydrofuran (untreated) was used as the mobile phase, the flow rate was 0.6 mL / min, and the elution curve of the resin was obtained. In order to calculate the average molecular weight and PDI of the resin, monodisperse polystyrene (PS) was used as the standard sample (12), and its molecular weight was 162, 445, 670, 1100, 2400, 3920, 5590, 7070, 10060, 18310, 29960 and 50800 g / mol respectively. The elution curve of the PS standard sample was measured, and the calibration curve of its molecular weight and retention time was obtained by fitting. The number average molecular weight, weight average molecular weight and PDI of the resin were calculated using the software provided by the instrument.

[0034] Example 1

[0035] Step 1, add BPM, a formaldehyde aqueous solution with a mass percentage concentration of 38.0%, ethanol and oxalic acid into a reaction kettle; wherein the molar ratio of BPM to formaldehyde is 1:0.95; the mass ratio of BPM to ethanol is 100:50; and the mass ratio of BPM to oxalic acid is 100:2;

[0036] Step 2: After purging with nitrogen, close the reactor, heat it to 100°C, control the pressure in the reactor to 0.110MPa, and keep the reaction at this temperature for 4 hours; heat it to 120°C, keep the reaction at this temperature for 4 hours, and control the pressure in the reactor to be no more than 0.2MPa;

[0037] Step 3: distill under normal pressure, pass nitrogen protection, raise the temperature to 140°C, remove most of the water and organic solvent; then distill under reduced pressure at 0.08MPa, heat the kettle to raise the temperature to 165°C, and maintain for 1.0h; finally, restore normal pressure, and cool the resin to 140°C under nitrogen protection;

[0038] Step 4: extracting the product of step 3 with xylene, the specific operation is as follows:

[0039] Add xylene to the reactor, pass nitrogen, stir at 60 rpm, heat to reflux (about 135°C), keep for 20 minutes, and then stop stirring; the mass ratio of xylene to BPM is 100:66.7; let it stand for 30 minutes, and after the xylene and resin in the reactor are separated, suck out the upper layer of xylene;

[0040] After repeating the above steps for 5 times, distill under reduced pressure at 140°C to remove xylene; discharge the material at 140°C under normal pressure to obtain a thermoplastic phenolic resin with a number average molecular weight of 1437 g / mol, a weight average molecular weight of 2363 g / mol, and a PDI of 1.64.

[0041] Example 2

[0042] Step 1, add BPM, a formaldehyde aqueous solution with a mass percentage concentration of 38.0%, ethanol and oxalic acid into a reaction kettle; wherein the molar ratio of BPM to formaldehyde is 1:1; the mass ratio of BPM to ethanol is 100:50; and the mass ratio of BPM to oxalic acid is 100:4;

[0043] Step 2: After purging with nitrogen, close the reactor, heat it to 90°C, control the pressure in the reactor to 0.108MPa, and keep the reaction at this temperature for 3 hours; heat it to 110°C, keep the reaction at this temperature for 3 hours, and control the pressure in the reactor to be no more than 0.2MPa;

[0044] Step 3: distill under normal pressure, pass nitrogen protection, raise the temperature to 130°C, remove most of the water and organic solvent; then distill under reduced pressure at -0.09MPa, heat to raise the temperature in the kettle to 162°C, and maintain for 0.8h; finally, restore normal pressure, and cool the resin to 135°C under nitrogen protection;

[0045] Step 4: extracting the product of step 3 with xylene, the specific operation is as follows:

[0046] Add xylene to the reactor, pass nitrogen, stir at 60 rpm, heat to reflux (about 135°C), keep stirring for 20 minutes, and stop stirring; the mass ratio of xylene to BPM is 100:200; let it stand for 30 minutes, and after the xylene and resin in the reactor are separated, suck out the upper layer of xylene;

[0047] After repeating the above steps twice, distill under reduced pressure at 140°C to remove xylene; discharge the material at 140°C under normal pressure to obtain a thermoplastic phenolic resin with a number average molecular weight of 1174 g / mol, a weight average molecular weight of 2239 g / mol, and a PDI of 1.91.

[0048] After the resin is cured by hexamethylenetetramine, the carbonization rate can reach up to 60.0%, the interlaminar shear strength of the carbon fiber reinforced composite material reaches 50MPa, and the linear ablation rate is 0.022mm / s.

[0049] Example 3

[0050] Step 1, add BPM, a 35.0% formaldehyde aqueous solution, ethanol and oxalic acid into a reaction kettle; wherein the molar ratio of BPM to formaldehyde is 1:1; the mass ratio of BPM to ethanol is 100:50; and the mass ratio of BPM to oxalic acid is 100:4;

[0051] Step 2: After purging with nitrogen, close the reactor, heat it to 85°C, control the pressure in the reactor to 0.110MPa, and keep the reaction at this temperature for 2h; heat it to 100°C, keep the reaction at this temperature for 2h, and control the pressure in the reactor to be no more than 0.2MPa;

[0052] Step 3: distill under normal pressure, pass nitrogen protection, raise the temperature to 130°C, remove most of the water and organic solvent; then distill under reduced pressure at -0.08MPa, and heat to raise the temperature in the kettle to 165°C, and maintain for 0.5h; finally, restore normal pressure, and cool the resin to 140°C under nitrogen protection;

[0053] Step 4: extracting the product of step 3 with xylene, the specific operation is as follows:

[0054] Add xylene to the reactor, pass nitrogen, stir at 100 rpm, heat to reflux (about 135°C), keep stirring for 30 minutes, and stop stirring; the mass ratio of xylene to BPM is 100:100; let it stand for 40 minutes, and after the xylene and resin in the reactor are separated, suck out the upper layer of xylene;

[0055] After repeating the above steps for 4 times, distill under reduced pressure at 140°C to remove xylene; discharge the material at 145°C under normal pressure to obtain a thermoplastic phenolic resin with a number average molecular weight of 1333 g / mol, a weight average molecular weight of 2430 g / mol, and a PDI of 1.82.

[0056] After the resin is cured by hexamethylenetetramine, the carbonization rate can reach up to 63.0%, the interlaminar shear strength of the carbon fiber reinforced composite material reaches 57MPa, and the linear ablation rate is 0.021mm / s.

[0057] Example 4

[0058] Step 1, add BPM, a 35.0% formaldehyde aqueous solution, tetrahydrofuran and oxalic acid into a reaction kettle; wherein the molar ratio of BPM to formaldehyde is 1:1; the mass ratio of BPM to tetrahydrofuran is 100:50; and the mass ratio of BPM to oxalic acid is 100:4;

[0059] Step 2: After purging with nitrogen, close the reactor, heat it to 85°C, control the pressure in the reactor to 0.110MPa, and keep the reaction at this temperature for 2h; heat it to 100°C, keep the reaction at this temperature for 2h, and control the pressure in the reactor to be no more than 0.2MPa;

[0060] Step 3: distill under normal pressure, pass nitrogen protection, raise the temperature to 130°C, remove most of the water and organic solvent; then distill under reduced pressure at -0.08MPa, and heat to raise the temperature in the kettle to 165°C, and maintain for 0.5h; finally, restore normal pressure, and cool the resin to 140°C under nitrogen protection;

[0061] Step 4: extracting the product of step 3 with xylene, the specific operation is as follows:

[0062] Add xylene to the reactor, pass nitrogen, stir at 50 rpm, heat to reflux (about 135°C), keep stirring for 20 minutes, and stop stirring; the mass ratio of xylene to BPM is 100:100; let it stand for 30 minutes, and after the xylene and resin in the reactor are separated, suck out the upper layer of xylene;

[0063] After repeating the above steps for 5 times, distill under reduced pressure at 140°C to remove xylene; discharge the material at 145°C under normal pressure to obtain a thermoplastic phenolic resin with a number average molecular weight of 1498 g / mol, a weight average molecular weight of 2680 g / mol, and a PDI of 1.79.

[0064] Example 5

[0065] Step 1, add BPM, a 35.0% formaldehyde aqueous solution, acetone and oxalic acid into a reaction kettle; wherein the molar ratio of BPM to formaldehyde is 1:0.8; the mass ratio of BPM to acetone is 100:80; the mass ratio of BPM to oxalic acid is 100:5;

[0066] Step 2: After purging with nitrogen, close the reactor, heat it to 85°C, control the pressure in the reactor to 0.110MPa, and keep the reaction at this temperature for 2h; heat it to 100°C, keep the reaction at this temperature for 2h, and control the pressure in the reactor to be no more than 0.2MPa;

[0067] Step 3: distill under normal pressure, pass nitrogen protection, raise the temperature to 130°C, remove most of the water and organic solvent; then distill under reduced pressure at -0.08MPa, and heat to raise the temperature in the kettle to 165°C, and maintain for 0.5h; finally, restore normal pressure, and cool the resin to 140°C under nitrogen protection;

[0068] Step 4: extracting the product of step 3 with xylene, the specific operation is as follows:

[0069] Add xylene to the reactor, pass nitrogen, stir at 50 rpm, heat to reflux (about 135°C), keep stirring for 30 minutes, and stop stirring; the mass ratio of xylene to BPM is 100:50; let it stand for 20 minutes, and after the xylene and resin in the reactor are separated, suck out the upper layer of xylene;

[0070] After repeating the above steps for 5 times, distill under reduced pressure at 140°C to remove xylene; discharge the material at 145°C under normal pressure to obtain thermoplastic phenolic resin.

[0071] Example 6

[0072] Step 1, add BPM, a formaldehyde aqueous solution with a mass percentage concentration of 35.0%, methanol and oxalic acid into a reactor; wherein the molar ratio of BPM to formaldehyde is 1:1.2; the mass ratio of BPM to methanol is 100:100; the mass ratio of BPM to oxalic acid is 100:0.5;

[0073] Step 2: After purging with nitrogen, close the reactor, heat it to 85°C, control the pressure in the reactor to 0.110MPa, and keep the reaction at this temperature for 2h; heat it to 100°C, keep the reaction at this temperature for 2h, and control the pressure in the reactor to be no more than 0.2MPa;

[0074] Step 3: distill under normal pressure, pass nitrogen protection, raise the temperature to 130°C, remove most of the water and organic solvent; then distill under reduced pressure at -0.08MPa, and heat to raise the temperature in the kettle to 165°C, and maintain for 0.5h; finally, restore normal pressure, and cool the resin to 140°C under nitrogen protection;

[0075] Step 4: extracting the product of step 3 with xylene, the specific operation is as follows:

[0076] Add xylene to the reactor, pass nitrogen, stir at 20 rpm, heat to reflux (about 135°C), keep for 10 minutes, and then stop stirring; the mass ratio of xylene to BPM is 100:150; let it stand for 30 minutes, and after the xylene and resin in the reactor are separated, suck out the upper layer of xylene;

[0077] After repeating the above steps for 6 times, distill under reduced pressure at 140°C to remove xylene; discharge the material at 135°C under normal pressure to obtain thermoplastic phenolic resin.

[0078] Comparative Example 1

[0079] Step 1, add BPM, a formaldehyde aqueous solution with a mass percentage concentration of 37.5.0%, ethanol and oxalic acid into a reaction kettle; wherein the molar ratio of BPM to formaldehyde is 1:0.95; the mass ratio of BPM to ethanol is 100:50; the mass ratio of BPM to oxalic acid is 100:2;

[0080] Step 2: After purging with nitrogen, close the reactor, heat it to 100°C, control the pressure in the reactor to 0.110MPa, and keep the reaction at this temperature for 4 hours; heat it to 120°C, keep the reaction at this temperature for 4 hours, and control the pressure in the reactor to be no more than 0.2MPa;

[0081] Step 3: distill at normal pressure, pass nitrogen protection, raise the temperature to 140°C, remove most of the water and organic solvents; then distill at reduced pressure at 0.08MPa, heat the kettle to raise the temperature to 165°C, and maintain for 1.0h; finally, restore normal pressure, cool the resin to 140°C under nitrogen protection, and obtain a resin with a number average molecular weight of 909g / mol, a weight average molecular weight of 1716g / mol, and a PDI of 1.89. The lower PDI indicates a narrower molecular weight distribution.

[0082] Comparative Example 2

[0083] Step 1, add BPM, a formaldehyde aqueous solution with a mass percentage concentration of 36.0%, ethanol and oxalic acid into a reaction kettle; wherein the molar ratio of BPM to formaldehyde is 1:1; the mass ratio of BPM to ethanol is 100:40; and the mass ratio of BPM to oxalic acid is 100:4;

[0084] Step 2: After purging with nitrogen, close the reactor, heat it to 80°C, control the pressure in the reactor to 0.105MPa, and keep the reaction at this temperature for 1h; heat it to 100°C, keep the reaction at this temperature for 1h, and control the pressure in the reactor to be no more than 0.2MPa;

[0085] Step 3: distill under normal pressure, pass nitrogen protection, raise the temperature to 120°C, remove most of the water and organic solvents; then distill under reduced pressure at -0.09MPa, heat the kettle to 160°C, and maintain for 0.2h; finally restore normal pressure, and cool the resin to 130°C under nitrogen protection. The number average molecular weight of the obtained resin is 880g / mol, the weight average molecular weight is 1869 / mol, and the PDI is 2.12.

[0086] Figure 11 is the GPC curve of the thermoplastic phenolic resin obtained in Example 1 and Comparative Example 1. In the figure, the peak on the right side of the GPC curve is formed by BPM in the resin. In Comparative Example 1, although the resin contains 16.10% BPM, it still has a low PDI, that is, PDI equals 1.89, indicating the effectiveness of the synthesis process of the present invention for synthesizing low PDI phenolic resin. In Example 1, since an extraction process is further adopted after the synthesis process, the low molecular weight part in the resin is reduced, especially BPM is reduced to 2.19%, resulting in a narrowing of the molecular weight distribution of the resin. Therefore, while the average molecular weight of the resin increases, its PDI is reduced to 1.64, indicating the effectiveness of the extraction process for reducing the PDI of the thermoplastic phenolic resin.

[0087] Figure 2 The GPC curves of the thermoplastic phenolic resin obtained in Comparative Example 2, Example 2, Example 3 and Example 4 are shown in FIG. In the figure, the peak on the right side of the GPC curve is formed by BPM in the resin. It can be seen from the corresponding peak that the content of BPM in Comparative Example 2 is the highest, and the content of BPM in Examples 2, 3 and 4 is reduced. According to the specific numerical analysis, in Comparative Example 2, the PDI of the resin is 2.12, and its BPM content is 19.13%. In Example 2, since an extraction process is further adopted after the synthesis process, the low molecular weight part in the resin is reduced, especially BPM is reduced to 8.07%, resulting in a narrowing of the molecular weight distribution of the resin, and therefore, its PDI is reduced to 1.91, indicating the effectiveness of the extraction process in reducing the PDI of the thermoplastic phenolic resin. In Example 3, the extraction process is further strengthened to reduce the BPM content in the resin to 4.47%, and its PDI is reduced to 1.82. In Example 4, the extraction process was further strengthened to reduce the BPM content in the resin to 2.67%, the molecular weight of the resin reached 2680 g / mol, and its PDI was reduced to 1.79. This shows the effectiveness of the synthesis process combined with the extraction process of the present invention in synthesizing low-PDI thermoplastic phenolic resin, especially the xylene extraction process is a process in which the average molecular weight increases and the PDI decreases.

Claims

1. A method for preparing a high molecular weight thermoplastic phenolic resin with a narrow molecular weight distribution, characterized in that: The following steps are involved: Step 1, adding dihydroxydiphenylmethane, formaldehyde aqueous solution, organic solvent and oxalic acid into a reaction kettle; wherein the molar ratio of dihydroxydiphenylmethane to formaldehyde is 1:(0.8-1.2); the mass ratio of dihydroxydiphenylmethane to organic solvent is 100:(40-100); the mass ratio of dihydroxydiphenylmethane to oxalic acid is 100:(0.5-5); the organic solvent includes an organic compound that is miscible with water and has good solubility in dihydroxydiphenylmethane; Step 2: After purging with nitrogen, close the reactor, heat it to 80-100°C, control the pressure in the reactor to 0.105-0.110 MPa, and keep the reaction at this temperature for 1-4 hours; heat it to 100-120°C, keep the reaction at this temperature for 1-4 hours, and control the pressure in the reactor to be no more than 0.2 MPa; Step 3: Pass nitrogen protection, raise the temperature to 120-140°C, perform atmospheric distillation to remove most of the water and organic solvents; then perform reduced pressure distillation at -0.09-0.08MPa, and heat the kettle to raise the temperature to 160-165°C, and maintain for 0.2-1.0h; finally, restore the normal pressure, and cool down to 130-140°C under nitrogen protection; Step 4: extracting the product of step 3 with xylene to obtain a high molecular weight thermoplastic phenolic resin with a narrow molecular weight distribution.

2. The method for preparing a high molecular weight thermoplastic novolac resin with a narrow molecular weight distribution as claimed in claim 1, characterized in that: The mass percentage concentration of the formaldehyde aqueous solution described in step 1 is 35.0-38.0%.

3. The method for preparing a high molecular weight thermoplastic novolac resin with a narrow molecular weight distribution as claimed in claim 1, characterized in that: The organic solvent includes any one of ethanol, methanol, acetone and tetrahydrofuran.

4. The method for preparing a high molecular weight thermoplastic novolac resin with a narrow molecular weight distribution as claimed in claim 1, characterized in that: The xylene described in step 4 includes any one of o-xylene, p-xylene or m-xylene, or a mixture of any proportions of the two or more of the o-xylene.

5. The method for preparing a high molecular weight thermoplastic novolac resin with a narrow molecular weight distribution as claimed in claim 1, characterized in that: The method of extracting the product of step 3 using xylene described in step 4 includes: S1: Add xylene to the reaction kettle, pass nitrogen, stir at a speed of 20-100 rpm, heat to reflux for 10-30 minutes, stop stirring, let stand for 20-40 minutes, and after the xylene and resin in the kettle are separated, suck out the upper layer of xylene; wherein the mass ratio of xylene to dihydroxydiphenylmethane is 100:(50-200); S2 repeats the operation of S1 2 to 6 times, and at the same time determines the molecular weight, distribution and composition of the resin by gel permeation chromatography. When the molecular weight of the resin reaches the requirement, the extraction process is completed; S3 is distilled under reduced pressure at 140°C to remove xylene, and discharged at 135-145°C under normal pressure to obtain a high molecular weight thermoplastic phenolic resin with a narrow molecular weight distribution.

6. A high molecular weight thermoplastic phenolic resin with narrow molecular weight distribution prepared by the method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Preparation method of phenolic resin having narrow molecular weight distribution

    CN102585124A

  • Preparation method of green high-purity thermoplastic phenolic resin

    CN104262557A

  • Thermoplastic phenolic resin with low bisphenol compound content as well as preparation method and application thereof

    CN110790876A

  • Novel hot melt adhesive and preparation method thereof

    CN112708376A

  • Expansion preparation method, production device and stability evaluation method of special phenolic resin with narrow distribution and wide processing window

    CN113278121A

Cited By

  • Resin prebaked anode and preparation method thereof

    CN121005569A

  • Resin prebaked anode and method for producing the same

    CN121005569B