Method for preparing regenerated polyesteramide based on ester-amide exchange reaction

Through the ester-amide exchange reaction method, the problems of harsh conditions and complex reactions in the recycling process of waste polyamide are solved, and low-energy consumption and high-efficiency preparation of recycled polyester amides are achieved, which simplifies operation and increases the added value and scope of application of the product. .

CN118878818AActive Publication Date: 2024-11-01DONGHUA UNIV

Patent Information

Application Number
CN202411130365.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-01
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

In the recycling process of waste polyamide, the existing technology has problems such as harsh conditions, complex reaction system, high equipment requirements and low molecular weight of recycled products, making it difficult to achieve efficient and concise resource reuse.

Method used

The ester-amide exchange reaction method is adopted to reduce the amino content in the middle of the molecular chain through esterification and capping, remove small molecule impurities such as dyes, achieve molecular chain growth, efficient extraction of effective components of polyamide, and omit the process of degradation to generate monomers. Reduce energy consumption and prepare high value-added regenerated polyester amides.

Benefits of technology

It realizes low-energy consumption and efficient preparation of recycled polyester amides, simplifies operations, reduces costs, is suitable for large-scale production, and increases the added value and scope of application of recycled products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997643380000121
    Figure BDA0004997643380000121
Patent Text Reader

Abstract

The invention relates to a method for preparing regenerated polyesteramide based on ester-amide exchange reaction. The method comprises the following steps: firstly, carrying out ester and amide exchange on waste polyamide to obtain a polyamide ester, then carrying out purification treatment on the polyamide ester to decolorize and remove impurities, and finally, carrying out dealcoholization through vacuum polycondensation to obtain regenerated polyesteramide. Compared with the prior art, the waste polyamide does not need to be depolymerized into the caprolactam monomer, energy consumption is low, reaction conditions are relatively mild, operation is easy, the method can be completed based on conventional reaction equipment, and the potential of large-scale production is achieved; the method realizes efficient recovery of waste polyamide and high value-added regeneration of polyesteramide, and provides technical support for cyclic utilization of waste polyamide textiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of recycling of waste textiles, and in particular to a method for preparing recycled polyester amide based on ester-amide exchange reaction. Background Art

[0002] Polyamide, also known as nylon, has excellent performance, good strength, wear resistance and elasticity, and is the second largest synthetic fiber in the textile field. However, with the rapid development of the polyamide textile industry, the amount of waste polyamide products (such as waste, scraps, discarded clothing, carpets, etc.) has increased year by year. Because it is difficult to degrade in the natural environment, it has brought great pressure to environmental protection. Therefore, developing efficient recycling technology to achieve the recycling of waste polyamide has become an important way to solve the above problems.

[0003] Since the components of polyamide materials are complex and generally contain plasticizers, pigments, functional additives, etc., there is a problem of difficulty in separation and purification during the recycling process. Although the most commonly used physical recycling method is simple and has low processing costs, the number of cycles that can be recycled through melt recycling is limited, and each cycle will cause micro-degradation of polyamide. Therefore, the quality of the recycled products is poor and the added value is low. Chemical recycling refers to the degradation of polyamide to form relatively low molecular weight and high value-added products. It is a recycling method with high potential value. However, the current methods of polyamide chemical recycling mainly use alcoholysis, aminolysis, hydrolysis and other means to depolymerize polyamide into monomers, and then apply the monomers to polyamide polymerization. These routes generally use high temperature and high pressure or supercritical conditions, and the monomer recovery rate is low, the energy consumption is large, and the requirements for reaction equipment are high.

[0004] Chinese patent CN117888223A discloses a method for preparing high-amino nylon 6 regenerated fiber, which uses nylon 6 mixed waste silk and terminal amino supplement Jinam-6 as raw materials, and obtains high-amino nylon 6 regenerated slices through operations such as crushing, melting plasticization, and pelletizing, and then melts the slices, spins them into yarn bundles, stretches them to shape them, and winds them to obtain finished products. However, this method belongs to the field of physical recycling, and the scope of application of the obtained regenerated fiber is limited.

[0005] Chinese patent CN113512193A discloses a method for alcoholysis regeneration of waste polyamide 6, which first adds an alkyd monomer to waste polyamide 6 under certain temperature and pressure conditions for alcoholysis to generate alcoholysis polyamide 6 segments with carboxyl and amino groups at both ends, then esterifies and amidates the segments under certain conditions to prepare regenerated polyamide 6, and uses a melt spinning method to prepare regenerated polyamide 6 fibers. However, this method is complicated to operate in the regeneration stage, and it is difficult to control the molecular weight of the polyamide 6 segments.

[0006] Chinese patent CN113248705A discloses a method and application for alcoholysis regeneration of waste polyester-polyamide 6 blended textiles, which uses alcoholysis of polyester-polyamide 6 blended textiles to obtain amide oligomers and polyester oligomers, which are then reacted with dibasic acids to prepare regenerated polyester amide. However, the reaction system is complex and the control requirements for the alcoholysis process are high.

[0007] It can be seen that the above existing technologies generally have problems such as harsh recycling conditions for waste polyamide, complex reaction system, high requirements for equipment, and low molecular weight of the recycled products. Therefore, in the context of increasingly serious plastic pollution, developing an efficient and simple resource recycling method for waste polyamide has become an important research direction in the textile field. Summary of the invention

[0008] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a method for preparing recycled polyester amide based on ester-amide exchange reaction, thereby providing an effective solution for recycling waste polyamide.

[0009] During the course of conception, the applicant believed that: the present invention firstly performs an ester-amide exchange reaction on waste polyamide to achieve esterification and end-capping, thereby reducing the content of terminal amino groups in the molecular chain, and then removes small molecular impurities such as dyes through purification processing, and finally achieves molecular chain growth by removing excess alcohol compounds, thereby omitting the process of degradation to generate monomers, reducing energy consumption, extracting the effective components of polyamide, and at the same time efficiently repolymerizing to prepare high value-added polyester amide.

[0010] The purpose of the present invention can be achieved by the following technical solutions:

[0011] A method for preparing recycled polyester amide based on ester-amide exchange reaction, the steps are as follows:

[0012] S1. Add waste polyamide and esterification product, ester exchange catalyst and heat stabilizer into a reaction vessel, introduce nitrogen to replace the air in the reactor, heat and stir to depolymerize, and obtain polyamide esterification product;

[0013] S2, decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester;

[0014] S3, placing the high-purity polyamide ester obtained in S2 in a reaction container, obtaining a regenerated polyester amide polymer by vacuum polycondensation, and then obtaining a regenerated polyester amide slice after cooling and drying;

[0015] S4, drying the regenerated polyester amide slices obtained in S3 and placing them in a melt spinning machine, and obtaining regenerated polyester amide fibers after melt spinning.

[0016] Furthermore, in S1, the weight ratio of the waste polyamide to the esterification product, the ester exchange catalyst, and the thermal stabilizer is 100:(1-50):(0.1-10):(0.1-10).

[0017] Furthermore, in S1, the waste polyamide is any one of polyamide 6, polyamide 66, and polyamide 56.

[0018] Furthermore, in S1, the esterified product is any one of ethylene terephthalate, 1,3-propylene terephthalate, 1,4-butylene terephthalate, ethylene isophthalate, 1,3-propylene isophthalate, and 1,4-butylene isophthalate.

[0019] Furthermore, in S1, the transesterification catalyst is any one of antimony trioxide, tetrabutyl titanate, isopropyl titanate, zinc acetate, manganese acetate, antimony acetate, and magnesium acetate.

[0020] Furthermore, in S1, the heat stabilizer is any one of triphenyl phosphate, triphenyl phosphite, Irganox 1010, Irganox 168, and Irganox 245.

[0021] Furthermore, in S1, the reaction temperature is 230-280° C., the pressure is 0.1-5 bar, the stirring speed is 50-500 r / min, and the stirring time is 1-3 h.

[0022] Furthermore, in S3, the reaction temperature is 240-280° C., the pressure is 0-100 Pa, and the reaction time is 2-4 h.

[0023] Furthermore, in S4, the specific steps of the melt spinning process include screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention is based on ester-amide exchange reaction. First, waste polyamide is subjected to ester-amide exchange reaction to achieve esterification and end-capping, reduce the content of terminal amino groups in the molecular chain, and remove small molecular impurities such as dyes rich in it through purification processing. Finally, the excess alcohol compounds are removed to achieve molecular chain growth. There is no need to depolymerize waste polyamide into caprolactam monomer, and the residual chemical additives and pigments and other impurities can be efficiently removed. The method has relatively mild reaction conditions, simple operation, low energy consumption, can efficiently extract the effective components of waste polyamide, and efficiently repolymerize to prepare high-value-added polyester amide, providing technical support for the establishment of a recycling system for waste polyamide textiles.

[0026] (2) The present invention can be completed based on conventional reaction equipment, has the characteristics of low cost and easy promotion, and has the potential for large-scale production. DETAILED DESCRIPTION

[0027] The present invention is described in detail below in conjunction with specific embodiments. Any features such as preparation means, materials, structures or composition ratios not clearly described in this technical solution are regarded as common technical features disclosed in the prior art.

[0028] In the present invention, unless otherwise specified, the detection method of each parameter is as follows.

[0029] Performance test of regenerated polyester amide fiber in various embodiments of the present invention:

[0030] (1) Strength: Under standard atmospheric conditions, use a constant rate elongation tester and calculate the strength according to the formula Calculate its strength, where σ is the breaking strength, in centinewtons per dtex (cN / dtex); F is the breaking strength of the sample, in centinewtons (cN); T is the linear density measured by the same laboratory sample, in dtex (dtex). For specific test principles and methods, see GB / T14344-2008.

[0031] (2) Elongation: Under standard atmospheric conditions, use a constant rate elongation tester and calculate the elongation according to the formula Calculate its elongation, where ε is the elongation at break, %; E is the elongation value, in millimeters (mm); L0 is the starting length, in millimeters (mm). For specific test principles and methods, see GB / T 14344-2008.

[0032] In each embodiment of the present invention, the "melt spinning machine" is a multifunctional flexible spinning machine, and the process parameters of melt spinning are: spinning temperature 250°C, spinneret temperature 260°C, screw pressure 6.5MPa, metering pump pressure 13MPa, spinning speed 2000m / min, and drafting multiple 3.0.

[0033] Example 1

[0034] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0035] S1. Add 100 g of waste polyamide 6, 1 g of ethylene terephthalate, 1 g of antimony trioxide and 3 g of triphenyl phosphate into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 245° C., depolymerize for 2 h at a pressure of 0.1 bar and a stirring speed of 280 r / min to obtain a polyamide ester.

[0036] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0037] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 240° C., while the pressure is reduced to 20 Pa, and the reaction is continued for 2 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0038] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.3 cN·dtex -1 , the elongation is 11%.

[0039] Example 2

[0040] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0041] S1. Add 100 g of waste polyamide 6, 5 g of 1,3-propylene terephthalate, 4 g of tetrabutyl titanate and 1 g of triphenyl phosphite into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 260°C, depolymerize at a pressure of 2 bar and a stirring speed of 380 r / min for 1.6 h to obtain a polyamide ester.

[0042] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0043] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 244° C., while the pressure is reduced to 50 Pa, and the reaction is continued for 2.8 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0044] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.5 cN·dtex -1 , the elongation is 14%.

[0045] The preparation method of "1,3-propylene terephthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of terephthalic acid) is added to terephthalic acid and 1,3-propylene glycol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,3-propylene terephthalate.

[0046] Example 3

[0047] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0048] S1. Add 100 g of waste polyamide 6, 10 g of 1,4-butylene terephthalate, 7 g of isopropyl titanate and 0.1 g of Irganox 1010 into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 275° C., depolymerize at a pressure of 5 bar and a stirring speed of 450 r / min for 1.2 h to obtain a polyamide ester.

[0049] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0050] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 248° C., while the pressure is reduced to 0 Pa, and the reaction is continued for 3.2 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0051] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.6 cN·dtex -1 , the elongation is 15%.

[0052] The preparation method of "1,4-butylene terephthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of terephthalic acid) is added to terephthalic acid and 1,4-butanediol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,4-butylene terephthalate.

[0053] Example 4

[0054] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0055] S1. Add 100 g of waste polyamide 6, 15 g of ethylene isophthalate, 10 g of zinc acetate and 5 g of Irganox 168 into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 280° C., depolymerize at a pressure of 4.2 bar and a stirring speed of 200 r / min for 1.8 h to obtain a polyamide ester.

[0056] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0057] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 252° C., while the pressure is reduced to 35 Pa, and the reaction is continued for 3.6 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0058] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.6 cN·dtex -1 , the elongation is 15%.

[0059] Example 5

[0060] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0061] S1. Add 100 g of waste polyamide 6, 20 g of 1,3-propylene isophthalate, 5 g of manganese acetate and 8 g of Irganox 245 into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 235° C., depolymerize at a pressure of 2.5 bar and a stirring speed of 470 r / min for 1 h to obtain a polyamide ester.

[0062] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0063] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction vessel, and the temperature is gradually increased to 256° C., while the pressure is reduced to 100 Pa, and the reaction is continued for 3.8 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0064] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.2 cN·dtex -1 , the elongation is 12%.

[0065] The preparation method of "1,3-propylene isophthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of isophthalic acid) is added to isophthalic acid and 1,3-propylene glycol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,3-propylene isophthalate.

[0066] Example 6

[0067] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0068] S1. Add 100 g of waste polyamide 6, 25 g of 1,4-butylene isophthalate, 0.1 g of antimony acetate and 10 g of triphenyl phosphate into a reaction container, introduce nitrogen to replace the air in the reactor, heat it to 270°C, depolymerize it at a pressure of 3.4 bar and a stirring speed of 500 r / min for 1.4 h to obtain a polyamide ester.

[0069] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0070] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 260° C., while the pressure is reduced to 80 Pa, and the reaction is continued for 3.9 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0071] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.7 cN·dtex -1 , the elongation is 16%.

[0072] The preparation method of "1,4-butylene isophthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of isophthalic acid) is added to isophthalic acid and 1,4-butanediol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,4-butylene isophthalate.

[0073] Example 7

[0074] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0075] S1. Add 100 g of waste polyamide 6, 30 g of ethylene terephthalate, 9 g of magnesium acetate and 6 g of triphenyl phosphite into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 250° C., depolymerize at a pressure of 1 bar and a stirring speed of 400 r / min for 2.2 h to obtain a polyamide ester.

[0076] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0077] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 264° C., while the pressure is reduced to 60 Pa, and the reaction is continued for 3 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0078] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.4 cN·dtex -1 , the elongation is 13%.

[0079] Example 8

[0080] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0081] S1. Add 100 g of waste polyamide 6, 34 g of 1,3-propylene terephthalate, 6 g of antimony trioxide and 9 g of Irganox 1010 into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 230° C., depolymerize at a pressure of 1.5 bar and a stirring speed of 100 r / min for 2.6 h to obtain a polyamide ester.

[0082] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0083] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 268° C., while the pressure is reduced to 30 Pa, and the reaction is continued for 2.4 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0084] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.4 cN·dtex -1 , the elongation is 13%.

[0085] The preparation method of "1,3-propylene terephthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of terephthalic acid) is added to terephthalic acid and 1,3-propylene glycol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,3-propylene terephthalate.

[0086] Example 9

[0087] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0088] S1. Add 100 g of waste polyamide 6, 38 g of 1,4-butylene terephthalate, 2 g of tetrabutyl titanate and 0.5 g of Irganox 168 into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 240° C., depolymerize at a pressure of 0.5 bar and a stirring speed of 50 r / min for 2.4 h to obtain a polyamide ester.

[0089] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0090] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 272° C., while the pressure is reduced to 70 Pa, and the reaction is continued for 2.2 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0091] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.5 cN·dtex -1 , the elongation is 14%.

[0092] The preparation method of "1,4-butylene terephthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of terephthalic acid) is added to terephthalic acid and 1,4-butanediol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,4-butylene terephthalate.

[0093] Example 10

[0094] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0095] S1. Add 100 g of waste polyamide 6, 42 g of ethylene isophthalate, 8 g of isopropyl titanate and 4 g of Irganox 245 into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 265° C., depolymerize at a pressure of 3.8 bar and a stirring speed of 250 r / min for 2.9 h to obtain a polyamide ester.

[0096] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0097] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 276° C., while the pressure is reduced to 40 Pa, and the reaction is continued for 3.4 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0098] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.7 cN·dtex -1 , the elongation is 16%.

[0099] Embodiment 11

[0100] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0101] S1. Add 100 g of waste polyamide 6, 48 g of 1,3-propylene isophthalate, 0.5 g of zinc acetate and 2 g of triphenyl phosphate into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 255°C, depolymerize for 3 hours at a pressure of 4.8 bar and a stirring speed of 150 r / min to obtain a polyamide ester.

[0102] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0103] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 280° C., while the pressure is reduced to 10 Pa, and the reaction is continued for 2.6 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0104] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.6 cN·dtex -1 , the elongation is 15%.

[0105] The preparation method of "1,3-propylene isophthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of isophthalic acid) is added to isophthalic acid and 1,3-propylene glycol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,3-propylene isophthalate.

[0106] Example 12

[0107] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0108] S1. Add 100 g of waste polyamide 6, 50 g of 1,4-butylene isophthalate, 3 g of manganese acetate and 7 g of triphenyl phosphite into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 270°C, depolymerize at a pressure of 3 bar and a stirring speed of 320 r / min for 2.8 h to obtain a polyamide ester.

[0109] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0110] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 272° C., while the pressure is reduced to 90 Pa, and the reaction is continued for 4 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0111] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.8 cN·dtex -1 , the elongation is 18%.

[0112] The preparation method of "1,4-butylene isophthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of isophthalic acid) is added to isophthalic acid and 1,4-butanediol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,4-butylene isophthalate.

[0113] Example 13

[0114] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0115] S1. Add 100 g of waste polyamide 6, 50 g of 1,4-butylene isophthalate, 3 g of manganese acetate and 7 g of triphenyl phosphite into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 250°C, depolymerize at a pressure of 3 bar and a stirring speed of 320 r / min for 2.8 h to obtain a polyamide ester.

[0116] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0117] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 272° C., while the pressure is reduced to 90 Pa, and the reaction is continued for 4 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0118] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.7 cN·dtex -1 , the elongation is 14%.

[0119] The preparation method of "1,4-butylene isophthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of isophthalic acid) is added to isophthalic acid and 1,4-butanediol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,4-butylene isophthalate.

[0120] Embodiment 14

[0121] This embodiment provides a method for preparing regenerated polyester amide based on ester-amide exchange reaction, comprising the following steps:

[0122] S1. Add 100 g of waste polyamide 6, 50 g of 1,4-butylene isophthalate, 3 g of manganese acetate and 7 g of triphenyl phosphite into a reaction container, introduce nitrogen to replace the air in the reactor, heat to 230°C, depolymerize at a pressure of 3 bar and a stirring speed of 320 r / min for 2.8 h to obtain a polyamide ester.

[0123] S2. Decolorizing, removing impurities and purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester.

[0124] S3. The high-purity polyamide ester obtained in step S2 is placed in a reaction container, and the temperature is gradually increased to 272° C., while the pressure is reduced to 90 Pa, and the reaction is continued for 4 hours under this condition. The obtained polymer is cooled and dried to obtain regenerated polyester amide chips.

[0125] S4, drying the regenerated polyester amide slices obtained in step S3 and placing them in a melt spinning machine, and then subjecting them to screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding to obtain regenerated polyester amide fibers. The strength of the regenerated polyester amide fiber is 4.6 cN·dtex -1 , the elongation is 14%.

[0126] The preparation method of "1,4-butylene isophthalate" in this embodiment is as follows: 0.05% tetrabutyl titanate (0.05% of the mass of isophthalic acid) is added to isophthalic acid and 1,4-butanediol (molar ratio 1:1.7), and esterification is carried out at 200°C for two hours to obtain 1,4-butylene isophthalate.

[0127] Table 1 Performance indexes of regenerated polyester amide fiber

[0128]

[0129] It can be seen from the data in Table 1 that Examples 1-14 provided by the present invention can efficiently and conveniently realize the recycling and regeneration of waste polyamide. The prepared regenerated polyester amide fiber has good physical properties and a strength of 4.2-4.8 cN·dtex. -1 , the elongation is 11-18%.

[0130] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing recycled polyester amide based on ester-amide exchange reaction, characterized in that: The following steps are involved: S1, heating and stirring waste polyamide, esterification product, ester exchange catalyst and heat stabilizer under nitrogen to depolymerize to obtain polyamide esterification product; S2, purifying the polyamide ester obtained in S1 to obtain a high-purity polyamide ester; S3, subjecting the high-purity polyamide ester obtained in S2 to vacuum polycondensation to obtain regenerated polyester amide, and then cooling and drying to obtain regenerated polyester amide slices; S4, subjecting the regenerated polyester amide slices obtained in S3 to melt spinning to obtain regenerated polyester amide fibers.

2. The method for preparing regenerated polyester amide based on ester-amide exchange reaction according to claim 1, characterized in that: In S1, the weight ratio of the waste polyamide to the esterification product, the ester exchange catalyst and the thermal stabilizer is 100:(1-50):(0.1-10):(0.1-10).

3. A method for preparing regenerated polyester amide based on ester-amide exchange reaction according to claim 1 or 2, characterized in that: In S1, the waste polyamide is any one of polyamide 6, polyamide 66, and polyamide 56.

4. A method for preparing regenerated polyester amide based on ester-amide exchange reaction according to claim 1 or 2, characterized in that: In S1, the esterified product is any one of ethylene terephthalate, 1,3-propylene terephthalate, 1,4-butylene terephthalate, ethylene isophthalate, 1,3-propylene isophthalate, and 1,4-butylene isophthalate.

5. A method for preparing regenerated polyester amide based on ester-amide exchange reaction according to claim 1 or 2, characterized in that: In S1, the transesterification catalyst is any one of antimony trioxide, tetrabutyl titanate, isopropyl titanate, zinc acetate, manganese acetate, antimony acetate, and magnesium acetate.

6. A method for preparing regenerated polyester amide based on ester-amide exchange reaction according to claim 1 or 2, characterized in that: In S1, the heat stabilizer is any one of triphenyl phosphate, triphenyl phosphite, Irganox 1010, Irganox 168, and Irganox 245.

7. The method for preparing regenerated polyester amide based on ester-amide exchange reaction according to claim 1, characterized in that: In S1, the reaction temperature is 230-280°C and the pressure is 0.1-5 bar.

8. The method for preparing regenerated polyester amide based on ester-amide exchange reaction according to claim 1, characterized in that: In S1, the stirring speed is 50-500 r / min, and the stirring time is 1-3 h.

9. The method for preparing regenerated polyester amide based on ester-amide exchange reaction according to claim 1, characterized in that: In S3, the reaction temperature is 240-280° C., the pressure is 0-100 Pa, and the reaction time is 2-4 h.

10. The method for preparing regenerated polyester amide based on ester-amide exchange reaction according to claim 1, characterized in that: In S4, the specific steps of the melt spinning process include screw extrusion melting, spinneret extrusion, side blowing cooling, bundling oiling, drawing, and winding.

Citation Information

Patent Citations

  • Caprolactam hydrolyzed polymer fibres and spinning method thereof

    CN104480561A

  • Recycled polyester as well as preparation method and application thereof

    CN114524924A

  • Polyesteramide, polyesteramide fiber and preparation method

    CN118165239A

  • Method for recycling and preparing regenerated polymer from waste mixed plastic and regenerated polymer

    CN118406282A

  • Recycled polyester using waste polyester and manufacturing method thereof

    KR1020120128480A

Cited By

  • Method for preparing degradable polyesteramide elastomer from waste chemical fibers

    CN120623474A

  • Method for recycling waste colored chinlon

    CN121628094A