Flexible high-conductivity PVC-based electromagnetic shielding composite film and preparation method thereof

The flexible high-conductive PVC-based electromagnetic shielding composite film was prepared by solvent hot pressing method, which solved the high cost and performance damage problems of high-temperature hot pressing and mechanical compression methods in the prior art, and achieved efficient and low-cost electromagnetic shielding film production.

CN118878884APending Publication Date: 2024-11-01THE 925TH HOSPITAL OF THE CHINESE PEOPLES LIBERATION ARMY JOINT LOGISTICS SUPPORT FORCE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411125882.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing carbon-based electromagnetic shielding composite film preparation methods include high-temperature hot pressing and mechanical compression methods, which have harsh production conditions, high cost and may damage conductive materials, affecting electromagnetic shielding performance.

Method used

The solvent hot pressing method is used to stir PVC and carbon nanofillers in a volatile solvent and then scrape them on the substrate. The solvent is volatile by natural covering and heating of the fabric, thereby achieving thin film forming and reducing production costs and equipment investment.

Benefits of technology

Improve electromagnetic shielding and conductive properties, simplify process flow, reduce production costs, and do not damage the conductive material structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878884A_ABST
    Figure CN118878884A_ABST
Patent Text Reader

Abstract

The invention discloses a flexible high-conductivity PVC-based electromagnetic shielding composite film and a preparation method thereof. The preparation method comprises the following steps: (1) dispersing PVC and the carbon nanofiller in a solvent, stirring and defoaming to obtain a membrane casting solution; (2) blade-coating the casting solution on a substrate; and (3) naturally covering cloth on the blade-coated membrane casting solution, then heating until the solvent is volatilized and phase inversion forming occurs, and by virtue of gravity extrusion of the cloth in the membrane forming process, reducing the thickness of the composite membrane, and improving the connectivity of a carbon nanofiller network and the content of the carbon nanofiller in unit volume, thereby obtaining the flexible high-conductivity PVC-based electromagnetic shielding composite membrane. The electromagnetic shielding film has the advantages of being high in electromagnetic shielding performance, simple in production process and low in cost, and has very good application prospects in the field of electromagnetic shielding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an electromagnetic shielding film and a preparation method thereof, in particular to a flexible high-conductive PVC-based electromagnetic shielding composite film and a preparation method thereof. Background Art

[0002] With the rapid development of 5G communication technology, the integration and application frequency of electronic devices have been continuously improved, and have spread to most scenes of people's lives and work. At the same time, their overall size is getting smaller and smaller, resulting in a large number of portable electronic devices. However, electronic devices are prone to some failures when exposed to high-frequency electromagnetic radiation for a long time. At the same time, high-frequency electromagnetic radiation can also cause certain harm to human health. Therefore, the development and application of high-performance electromagnetic shielding materials is one of the important means to solve the hazards of electromagnetic radiation.

[0003] In recent years, carbon-based composite electromagnetic shielding films have attracted intensive attention due to their corrosion resistance, low thickness and high stability. At the same time, these highly conductive composite films made of conductive materials such as carbon nanotubes and graphene and high molecular polymers have shown excellent electromagnetic shielding performance.

[0004] However, in order to obtain a thinner electromagnetic shielding film, the current preparation methods of carbon-based electromagnetic shielding composite films mostly use high-temperature hot pressing and mechanical compression methods for production. The former is to press the cast film material in the mold into a film under high temperature conditions, while the latter is to use mechanical force to compress the thicker film to prepare the required thinner electromagnetic shielding film. The problems with these two methods are: the high-temperature hot pressing method needs to be carried out at a high temperature, the production conditions are relatively harsh, and the production cost is high, while the mechanical compression method requires the use of compression equipment, which increases the equipment cost on the one hand, and at the same time, mechanical compression will destroy the structure of conductive materials such as carbon nanotubes, thereby affecting the conductive performance and reducing the electromagnetic shielding effect.

[0005] The patent name is a method for preparing a flexible conductive PVC-based composite film, and the publication number is CN115662679A. It specifically discloses a method for obtaining a flexible conductive PVC-based composite film by mixing PVC and two different diluents, adding nano-carbon materials to make a casting liquid, then coating the casting liquid on a non-woven fabric and solidifying it, and finally extracting it. The composite film obtained by this method has high conductivity and is also a flexible film. Therefore, it can be used as an electromagnetic shielding film according to conventional understanding. However, since it needs to be extracted and heat treated during preparation to obtain high conductivity, the preparation process is relatively complicated and the cost is also high.

[0006] Therefore, in order to reduce the production cost of electromagnetic shielding film, reduce equipment investment, make the process easy to operate, and ensure the electromagnetic shielding performance of the electromagnetic shielding film, the researchers of this application studied and improved the composition and preparation method of the electromagnetic shielding film. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a flexible high-conductive PVC-based electromagnetic shielding composite film and a preparation method thereof. The electromagnetic shielding film of the present invention has the characteristics of strong electromagnetic shielding performance, simple production process and low cost.

[0008] The technical solution of the present invention:

[0009] A method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film comprises the following steps:

[0010] (1) dispersing PVC and carbon nanofiller in a solvent, stirring and degassing to obtain a casting solution;

[0011] (2) applying the casting solution onto the substrate;

[0012] (3) The cloth is naturally covered on the coated casting liquid, and then heated until the solvent evaporates and phase transformation occurs to obtain a flexible and highly conductive PVC-based electromagnetic shielding composite film.

[0013] Preferably, in the aforementioned method for preparing the flexible and highly conductive PVC-based electromagnetic shielding composite film, in the casting solution, the solid content of PVC is 70-99%, and the solid content of the carbon nanofiller is 1-30%.

[0014] Preferably, in the aforementioned method for preparing the flexible and highly conductive PVC-based electromagnetic shielding composite film, the solvent is any one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, triethyl phosphate, trimethyl phosphate and dimethyl sulfoxide.

[0015] Preferably, in the method for preparing the aforementioned flexible high-conductive PVC-based electromagnetic shielding composite film, the stirring in step (1) is carried out at 25-80° C. for 6-24 hours.

[0016] Preferably, in the method for preparing the aforementioned flexible highly conductive PVC-based electromagnetic shielding composite film, the scraping in step (2) is performed using a scraper with a size of 100-5000 μm at a speed of 1.0-5.0 m / s.

[0017] Preferably, in the aforementioned method for preparing the flexible and highly conductive PVC-based electromagnetic shielding composite film, the average thickness of the scraping in step (2) is 400-1000 μm.

[0018] Preferably, in the aforementioned method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film, the fabric in step (3) is any one of polyethylene terephthalate nonwoven fabric, polyamide nonwoven fabric and knitted fabric.

[0019] Preferably, in the method for preparing the aforementioned flexible high-conductive PVC-based electromagnetic shielding composite film, the weight of the fabric in step (3) is 80-220 g / m 2 .

[0020] Preferably, in the aforementioned method for preparing the flexible and highly conductive PVC-based electromagnetic shielding composite film, the heating temperature in step (3) is 30-80°C.

[0021] A flexible and highly conductive PVC-based electromagnetic shielding composite film prepared according to the aforementioned method.

[0022] Beneficial effects of the present invention:

[0023] The electromagnetic shielding composite film of the present invention is prepared by compression molding with a volatile solvent and a cloth of a certain weight. The present invention calls it solvent hot pressing method, that is, under the compression of the cloth's own gravity, the PVC and carbon nanofillers in the casting liquid are continuously squeezed in the direction of gravity, and as the volatile solvent therein continues to evaporate, the thickness of the composite film will be further compressed and thinned, increasing the density of the material, so that the content of carbon nanofillers per unit volume of the composite film is increased, and the connectivity of the conductive network of the bottom film is improved, thereby improving the conductive performance and electromagnetic shielding performance of the bottom film. Compared with the traditional high-temperature hot pressing method, mechanical compression method, solvent extraction and heat treatment method, it has lower cost and simpler process.

[0024] In summary, the electromagnetic shielding film of the present invention has the advantages of strong electromagnetic shielding performance, simple production process and low cost, and has very good application prospects in the field of electromagnetic shielding. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Attached Figure 1 This is a SEM image of the composite membrane prepared in Example 1 of the present invention;

[0026] Attached Figure 2 is the SEM image of the composite membrane prepared in comparative case 1;

[0027] Attached Figure 3 TEM image of the composite film prepared in comparative case 1;

[0028] Attached Figure 4 TEM image of the composite film prepared in comparative case 2;

[0029] pass Figure 1 and Figure 2It can be seen that the solvent hot pressing method can reduce the thickness of the film and improve the connectivity between the carbon nanofillers in the composite film, which is beneficial to improve the connectivity of the conductive network of the composite film, and then it is beneficial to improve the conductive performance and electromagnetic shielding performance of the composite film. In order to reveal that the solvent hot pressing method is more effective in optimizing the conductive network than the traditional method, we performed TEM characterization on the composite film of the implementation case 2 and the comparative case 1. It can be clearly observed from the figure that the network structure of the carbon nanofillers in the composite film is completely different. Among them, the composite film prepared by the solvent hot pressing method presents a highly connected state of carbon nanofillers, while the carbon nanofillers in the composite film prepared by the traditional method have poor connectivity. These experimental results can show that the method of the present invention has the effect of reducing the thickness of the film and optimizing the conductive network structure. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.

[0031] Embodiments of the present invention

[0032] The carbon nanofiller used in the examples and comparative examples of the present invention is CNT, and other carbon nanofillers of the same type can be directly applied to the present invention.

[0033] Example 1

[0034] A method for preparing a highly conductive PVC-based electromagnetic shielding composite film comprises the following steps:

[0035] (1) Preparation of casting solution: PVC with a solid content of 70% and CNT with a solid content of 30% were dispersed in N,N-dimethylformamide, and vacuum degassed at a temperature of 70°C after mechanical stirring for 10 hours to prepare a PVC / CNT casting solution;

[0036] (2) Scraping the casting liquid: Use a scraper with a size of 100 μm, scrape at a speed of 5.0 m / s, set the scraping thickness to 400 μm, and scrape the above PVC / CNT casting liquid onto the glass plate with a scraper;

[0037] (3) Solvent hot pressing and phase inversion molding: The PVC / CNT film casting liquid coated on the glass plate was subjected to solvent hot pressing. Specifically, the PVC / CNT film casting liquid with a gram weight of 80 g / m 2 The polyethylene terephthalate nonwoven fabric is laid flat on the PVC / CNT casting solution and placed in an oven at 60°C for solvent evaporation and phase conversion molding.

[0038] Example 2

[0039] A method for preparing a highly conductive PVC-based electromagnetic shielding composite film comprises the following steps:

[0040] (1) Preparation of casting solution: PVC with a solid content of 95% and CNT with a solid content of 5% were dispersed in N,N-dimethylacetamide, and vacuum degassed at a temperature of 70°C after mechanical stirring for 12 hours to prepare a PVC / CNT casting solution;

[0041] (2) Scraping the casting liquid: Use a scraper with a size of 1000 μm, scrape at a speed of 4.0 m / s, set the scraping thickness to 600 μm, and scrape the above PVC / CNT casting liquid onto the glass plate with a scraper;

[0042] (3) Solvent hot pressing and phase inversion molding: The PVC / CNT film casting liquid coated on the glass plate was subjected to solvent hot pressing. Specifically, the PVC / CNT film casting liquid with a gram weight of 85 g / m 2 The polyethylene terephthalate nonwoven fabric is laid flat on the PVC / CNT casting solution and placed in an oven at 30°C for solvent evaporation and phase conversion molding.

[0043] Example 3

[0044] A method for preparing a highly conductive PVC-based electromagnetic shielding composite film comprises the following steps:

[0045] (1) Preparation of casting solution: PVC with a solid content of 85% and CNT with a solid content of 15% were dispersed in N-methylpyrrolidone, and vacuum degassed at a temperature of 60° C. after mechanical stirring for 18 h to prepare a PVC / CNT casting solution;

[0046] (2) Scraping the casting liquid: Use a scraper with a size of 2000 μm, scrape at a speed of 3.0 m / s, set the scraping thickness to 800 μm, and scrape the above PVC / CNT casting liquid onto the glass plate with a scraper;

[0047] (3) Solvent hot pressing and phase inversion molding: The PVC / CNT film casting liquid coated on the glass plate was subjected to solvent hot pressing. Specifically, the PVC / CNT film casting liquid with a gram weight of 120 g / m 2 The polyamide nonwoven fabric is laid flat on the PVC / CNT casting solution and placed in an oven at 80°C for solvent evaporation and phase conversion molding.

[0048] Example 4

[0049] A method for preparing a highly conductive PVC-based electromagnetic shielding composite film comprises the following steps:

[0050] (1) Preparation of casting solution: PVC with a solid content of 85% and CNT with a solid content of 15% were dispersed in triethyl phosphate, and vacuum degassed at a temperature of 50° C. after mechanical stirring for 24 hours to prepare a PVC / CNT casting solution;

[0051] (2) Scraping the casting liquid: Use a scraper with a size of 4000 μm, scrape at a speed of 2.0 m / s, set the scraping thickness to 900 μm, and scrape the above PVC / CNT casting liquid onto the glass plate with a scraper;

[0052] (3) Solvent hot pressing and phase inversion molding: The PVC / CNT film casting liquid coated on the glass plate was subjected to solvent hot pressing. Specifically, the PVC / CNT film casting liquid with a gram weight of 200 g / m 2 The knitted fabric is laid flat on the PVC / CNT casting liquid and placed in an oven at 70°C for solvent evaporation and phase transformation molding.

[0053] Example 5

[0054] A method for preparing a highly conductive PVC-based electromagnetic shielding composite film comprises the following steps:

[0055] (1) Preparation of casting solution: PVC with a solid content of 99% and CNT with a solid content of 1% were dispersed in dimethyl sulfoxide, and vacuum degassed at a temperature of 60° C. after mechanical stirring for 18 h to prepare a PVC / CNT casting solution;

[0056] (2) Scraping the casting liquid: Use a scraper with a size of 5000 μm, scrape at a speed of 1.0 m / s, set the scraping thickness to 1000 μm, and scrape the above PVC / CNT casting liquid onto the glass plate with a scraper;

[0057] (3) Solvent hot pressing and phase inversion molding: The PVC / CNT film casting liquid coated on the glass plate was subjected to solvent hot pressing. Specifically, the PVC / CNT film casting liquid with a gram weight of 120 g / m 2 The polyamide nonwoven fabric is laid flat on the PVC / CNT casting solution and placed in an oven at 60°C for solvent evaporation and phase conversion molding.

[0058] Comparative case 1:

[0059] (1) Preparation of casting solution: PVC with a solid content of 95% and CNT with a solid content of 5% were dispersed in N,N-dimethylacetamide, and vacuum degassed at a temperature of 70°C after mechanical stirring for 12 hours to prepare a PVC / CNT casting solution;

[0060] (2) Scraping the casting liquid: Set the scraping thickness to 600 μm, and scrape the above PVC / CNT casting liquid onto the glass plate using a scraping machine;

[0061] (3) Solvent evaporation phase transformation molding: The PVC / CNT casting liquid coated on the glass plate was placed in an oven at 60°C for solvent evaporation phase transformation molding.

[0062] The electromagnetic shielding film obtained in this comparative case does not use natural compression of the fabric.

[0063] Comparative Case 2:

[0064] (1) Preparation of casting solution: PVC with a solid content of 95% and CNT with a solid content of 5% were dispersed in N,N-diethylformamide, and vacuum degassed at a temperature of 70°C after mechanical stirring for 12 hours to prepare a PVC / CNT casting solution;

[0065] (2) Scraping the casting liquid: Set the scraping thickness to 600 μm, and scrape the above PVC / CNT casting liquid onto the glass plate using a scraping machine;

[0066] (3) Solvent evaporation phase transformation molding: The PVC / CNT casting solution coated on the glass plate was placed in an oven at 60°C for solvent evaporation phase transformation molding;

[0067] (4) Mechanical hot pressing: The composite film was hot pressed at 200°C and 2 MPa for 30 minutes using a molding machine to prepare a sample with a thickness of 0.58 mm.

[0068] The electromagnetic shielding film obtained in this comparative case is a film processed by a conventional mechanical hot pressing method.

[0069] The conductive properties and electromagnetic shielding properties of the composite films provided by Examples 1-5 and Comparative Examples 1 and 2 are shown in Table 1.

[0070] Table 1 Comparison of the electrical conductivity and electromagnetic shielding properties of the composite films

[0071]

[0072] It can be seen from Table 1 that the electrical conductivity and electromagnetic shielding performance of the composite film can be significantly improved by solvent hot pressing; compared with mechanical hot pressing, the composite film prepared by this method has better electrical conductivity and electromagnetic shielding performance. In addition, when the CNT content is the same, the smaller the film thickness of the composite film treated by solvent hot pressing, the higher its electrical conductivity and electromagnetic shielding performance. In addition, through implementation cases 1-5, it can be seen that the electrical conductivity and electromagnetic shielding performance of the composite film are closely related to the CNT content. The higher the CNT content, the better the electrical conductivity and electromagnetic shielding performance of the obtained composite film.

[0073] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film, characterized in that: The steps include: (1) dispersing PVC and carbon nanofiller in a solvent, stirring and degassing to obtain a casting solution; (2) applying the casting solution onto the substrate; (3) The cloth is naturally covered on the coated casting liquid, and then heated until the solvent evaporates and phase transformation occurs to obtain a flexible and highly conductive PVC-based electromagnetic shielding composite film.

2. The method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film according to claim 1, characterized in that: In the casting solution, the solid content of PVC is 70-99%, and the solid content of carbon nano filler is 1-30%.

3. The method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film according to claim 1, characterized in that: The solvent is any one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, triethyl phosphate, trimethyl phosphate and dimethyl sulfoxide.

4. The method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film according to claim 1, characterized in that: The stirring in step (1) is carried out at 25-80° C. for 6-24 hours.

5. The method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film according to claim 1, characterized in that: The scraping in step (2) is performed using a scraper with a size of 100-5000 μm at a speed of 1.0-5.0 m / s.

6. The method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film according to claim 1, characterized in that: The average thickness of the scraping in step (2) is 400-1000 μm.

7. The method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film according to claim 1, characterized in that: The fabric in step (3) is any one of polyethylene terephthalate nonwoven fabric, polyamide nonwoven fabric and knitted fabric.

8. The method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film according to claim 1, characterized in that: The weight of the fabric in step (3) is 80-220 g / m 2 .

9. The method for preparing a flexible and highly conductive PVC-based electromagnetic shielding composite film according to claim 1, characterized in that: The heating temperature in step (3) is 30-80°C.

10. A flexible and highly conductive PVC-based electromagnetic shielding composite film prepared according to the method according to any one of claims 1 to 9.