Composite tread rubber elastomer and preparation method thereof

Through the blending of modified silicone rubber and styrene butadiene rubber and the use of high-efficiency vulcanizing agent, the problem of insufficient compatibility and mismatch of vulcanization speed in the tread glue is solved, and the mechanical properties and bonding strength of the tread glue are improved, so as to achieve The effective combination of tread glue and bottom glue.

CN118878950APending Publication Date: 2024-11-01CHENGDU GUIBAO SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411165258.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The compatibility between silicone rubber and styrene butadiene rubber in the existing tread rubber is insufficient, resulting in low mechanical strength, high Aclone wear, and the vulcanization speed of the tread rubber and the bottom rubber, resulting in a decrease in bonding strength.

Method used

Using silicone rubber modified styrene butadiene rubber, by increasing white carbon black and compatibilizer, the blending efficiency and compatibility of silicone rubber and styrene butadiene rubber is improved, and high-efficiency peroxide vulcanizing agent is used to coordinate vulcanization to match the tread. Vulcanization rate of glue and bottom glue.

Benefits of technology

The mechanical strength and wear resistance of the tread glue are improved, the combined strength of the tread glue and the bottom glue is enhanced, and the vulcanization speed of the tread glue and the bottom glue is matched, and the tread glue is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007687820000041
    Figure BDA0005007687820000041
  • Figure BDA0005007687820000051
    Figure BDA0005007687820000051
  • Figure BDA0005007687820000081
    Figure BDA0005007687820000081
Patent Text Reader

Abstract

The invention discloses a composite tread rubber elastomer and a preparation method thereof, and the composite tread rubber elastomer comprises the following components by mass: 100 parts of styrene butadiene rubber; 30 to 70 parts of white carbon black; 10 to 30 parts of silicone rubber compound; 5 to 10 parts of natural rubber; 5-10 parts of butadiene rubber; 1-5 parts of a coupling agent, 1-3 parts of an anti-aging agent, 1-3 parts of an assistant vulcanizing agent and 1-4 parts of a vulcanizing agent. The silicone rubber is mixed in advance, and the compatibilizer is added during mixing, so that the problem of poor compatibility of the silicone rubber and the styrene-butadiene rubber is solved, and meanwhile, the problem that the vulcanization speeds of the tread rubber and the primer rubber are not matched is solved by adopting the peroxide vulcanizing agent. The composite tread rubber elastomer is excellent in comprehensive performance, tensile strength is larger than or equal to 15 Mpa, elongation at break is larger than or equal to 500%, Akron abrasion is smaller than or equal to 0.15 cm < 3 > / 1.61 km, and aging resistance is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of tire rubber product manufacturing, and specifically relates to a novel composite tread rubber elastomer and a preparation method thereof. Background Art

[0002] The tread rubber is the outermost layer of the tire that contacts the road and has patterns printed on the surface. It gives the tire traction, cushions impact and swaying during driving, and prevents the cord layer from being cut or punctured. The base rubber refers to the rubber part under the tread rubber and on both sides of the tread rubber. The base rubber is mainly made of styrene-butadiene rubber, natural rubber, butadiene rubber and other rubbers.

[0003] The types of rubber raw materials used in tire tread rubber are mainly natural rubber and petroleum-based synthetic rubber (such as styrene-butadiene rubber), and the mixed rubber is required to have excellent wear resistance, anti-slip performance, aging resistance, mechanical properties, and low rolling resistance. In addition to its considerable output and independence from petroleum resources, silicone rubber also has excellent properties such as high and low temperature resistance, aging resistance, ozone resistance, and weather resistance. It can be used for a long time in the range of -100 to 250°C and has stable performance. It is expected to be used in the field of tires so that tires can obtain some excellent performance or improve the problems of traditional tires. Document CN105482200A discloses a high-wear-resistant and low-rolling-resistance tread rubber containing silicone rubber and a preparation method thereof. Silicone rubber is applied to tread rubber to improve wear resistance, and polythiol compounds are added during the mixing process of silicone rubber and styrene-butadiene rubber. The mercapto group of the polythiol compound reacts with the double bonds in silicone rubber and styrene-butadiene rubber under shear conditions, respectively, to achieve dynamic reaction volume expansion of silicone rubber and styrene-butadiene rubber, improve the mechanical properties of the rubber and reduce rolling resistance. However, this technology still has the following problems:

[0004] (1) Although the use of polythiols has improved the compatibility of silicone rubber and styrene-butadiene rubber to a certain extent, during the rubber refining process, the Mooney viscosity ML (1+4) of silicone rubber at 100°C is 3, while the Mooney viscosity ML (1+4) of styrene-butadiene rubber at 100°C is 50. Since the Mooney viscosity of silicone rubber is much lower than that of styrene-butadiene rubber, the solubility parameters of the two are quite different, resulting in insufficient compatibility between silicone rubber and styrene-butadiene rubber. The rubber compound has problems such as low blending efficiency and uneven filler dispersion, resulting in low mechanical strength of the tread rubber after blending, which limits the application of this rubber compound. (2) The sulfur vulcanization system and the peroxide vulcanization system are used together. The experimental results show that the vulcanization effects of the two are not ideal, the mechanical strength is lower than that of using a single vulcanizer, and the Akron wear is higher than that of using a single vulcanizer.

[0005] During the tire manufacturing process, the tread rubber and the tire base rubber will be vulcanized together, and the vulcanization temperature is generally around 155℃~170℃. The tread rubber uses traditional peroxide vulcanizers, such as diisopropylbenzene peroxide (DCP), 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane (bis-2,5), benzoyl peroxide, etc. Under this vulcanization temperature condition, the half-life of DCP and bis-2,5 is relatively long (the positive vulcanization time T90 is generally around 12~15min), and the half-life of benzoyl peroxide is relatively short (the positive vulcanization time T90 is generally around 2~3min); while the positive vulcanization time T90 of the tire base rubber is generally 5~7min. Therefore, the vulcanization speed of the tread rubber using traditional peroxide vulcanizers is too slow or too fast relative to the tire base rubber. The vulcanization speed of the tread rubber and the tire base rubber does not match during the co-vulcanization process, resulting in a decrease in the bonding strength between the two, which easily causes the tread rubber to fall off. Summary of the invention

[0006] Traditional tread rubber and silicone rubber are expected to partially replace natural rubber or petroleum-based synthetic rubber (such as styrene-butadiene rubber) in tread rubber by re-adjusting the formula, and give full play to the advantages of the two types of rubber to blend rubber with better performance to improve the performance of tread rubber. If this substitution can be achieved, the self-sufficiency rate of rubber will be greatly improved, bringing sufficient economic benefits and good social benefits to the development of the silicone industry.

[0007] In order to achieve the purpose of solving the problems of low mechanical strength of tread rubber containing silicone rubber, high Akron wear, and mismatch of vulcanization speed of tread rubber and tire base rubber, the present invention provides a composite tread rubber and a preparation method thereof, and uses silicone rubber to modify traditional styrene-butadiene rubber, which not only improves the blending efficiency of silicone rubber and styrene-butadiene rubber, solves the compatibility problem of silicone rubber and styrene-butadiene rubber, but also further improves the wear resistance and aging resistance of the tread rubber, and improves the mechanical strength of the tread rubber. At the same time, the present invention synthesizes a high-efficiency peroxide vulcanizing agent, applies it to the tread rubber blending process, solves the problem that the vulcanization speed of the tire base rubber and the composite tread rubber containing silicone rubber is difficult to match, and improves the bonding strength of the tread rubber and the tire base rubber.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A composite tread rubber elastomer comprises the following components in parts by weight:

[0010] Styrene butadiene rubber, 100 parts;

[0011] Silicone rubber compound, 10-30 parts;

[0012] Natural rubber, 5-10 parts;

[0013] Butadiene rubber, 5-10 parts;

[0014] White carbon black, 30-70 parts;

[0015] Coupling agent, 1 to 5 parts;

[0016] Anti-aging agent, 1 to 3 parts;

[0017] Vulcanizing agent, 1 to 3 parts;

[0018] Vulcanizing agent, 1 to 4 parts.

[0019] Furthermore, the styrene butadiene rubber is solution polymerized styrene butadiene rubber.

[0020] Furthermore, the silica component used in the composite tread rubber elastomer is at least one of precipitated silica and fumed silica.

[0021] Furthermore, the natural rubber is No. 1 standard rubber, and the brand of the butadiene rubber is BR9000. The present invention uses natural rubber and butadiene rubber to partially replace the styrene-butadiene rubber in the tread rubber, further improving the compatibility and bonding performance of the tread rubber and the tire base rubber.

[0022] Furthermore, the silicone rubber compound comprises the following components calculated by weight:

[0023] Methyl vinyl silicone rubber: 100 parts;

[0024] White carbon black: 20-50 parts;

[0025] Hydroxyl silicone oil: 2-5 parts

[0026] Compatibility enhancer: 1 to 5 parts.

[0027] Furthermore, the methyl vinyl silicone rubber used in the silicone rubber compound has a number average molecular weight of 350,000 to 650,000 and a vinyl content of 0.05% to 5%.

[0028] Furthermore, the viscosity of the hydroxy silicone oil used in the silicone rubber compound is 30-60 mPa.s (25° C.).

[0029] Furthermore, the compatibilizer used in the silicone rubber compound is trimethylolpropane-tris(3-mercaptopropionate). This compatibilizer uses its three mercapto groups to react with silicone rubber and styrene-butadiene rubber respectively, realizes in-situ reaction compatibilization during the blending process, and improves the compatibility of the silicone rubber and styrene-butadiene rubber mixed rubber. As one of the components of the silicone rubber compound, the compatibilizer is added when mixing the silicone rubber, so that the mercapto group and the silicone rubber are fully contacted and dispersed. When the silicone rubber and styrene-butadiene rubber are mixed, the mercapto group of the compatibilizer on the silicone rubber fully reacts with the styrene-butadiene rubber, thereby effectively improving the compatibility of the two phases of the mixed rubber.

[0030] Furthermore, the white carbon black is fumed white carbon black.

[0031] Since the Mooney viscosity of silicone rubber is 3(1+4)100℃, which is much lower than the Mooney viscosity of 50(1+4)100℃ of styrene-butadiene rubber, the solubility parameters of the two are quite different and the compatibility is poor. Therefore, we added white carbon black, compatibilizer, etc. to silicone rubber to increase the Mooney viscosity of the rubber. According to the principle of similarity when polymers are blended, when the viscosities of the two phases of polymers are close, the polymer blending is most efficient, the blending effect is best, and the dispersed phase size is smallest, which improves the "segregation" phenomenon of white carbon black in the two phases of silicone rubber and styrene-butadiene rubber and improves the compatibility of the two.

[0032] Optionally, the method for preparing the silicone rubber compound comprises the following steps:

[0033] Methyl vinyl silicone rubber, white carbon black, hydroxy silicone oil and compatibilizer are put into a kneading machine for mixing. After forming a mass, vacuum is drawn at 115-125°C for at least 1 hour to obtain a silicone rubber compound. After the silicone rubber compound is kneaded, the mill is opened to produce sheets for use. Optionally, vacuum is drawn at 120°C for 1 hour.

[0034] Furthermore, the coupling agent used in the composite tread rubber elastomer is at least one of bis-[γ-(triethoxysilyl)propyl]tetrasulfide, γ-methacryloxypropyltrimethoxysilane, and vinyltriethoxysilane.

[0035] Furthermore, the vulcanizing agent used in the composite tread rubber elastomer is at least one of trimethylolpropane trimethacrylate, triallyl isocyanurate, and ethylene glycol diacrylate.

[0036] Furthermore, the antioxidant used in the composite tread rubber elastomer is at least one of N-isopropyl-N'-phenyl-p-phenylenediamine and 2,2,4-trimethyl-1,2-dihydroquinoline polymer.

[0037] The present invention synthesizes a peroxide vulcanizing agent and uses it in conjunction with a co-vulcanizing agent to make the positive vulcanization time of the tread rubber and the positive vulcanization time of the tire base rubber close to each other, thereby improving the bonding performance of the tread rubber and the tire base rubber. The vulcanizing agent used in the composite tread rubber elastomer is a peroxide vulcanizing agent, and the structural formula of the peroxide vulcanizing agent is shown in formula (1):

[0038]

[0039] Where R is -C(CH 3 ) 3 or -CH 2 C(CH) 3 .

[0040] Optionally, the synthesis steps of the peroxide vulcanizing agent are as follows:

[0041]

[0042] 3,5-dimethylcyclohexanone (39.3 g, 0.4 mol) and tert-amyl hydroperoxide (128.7 g, 1.0 mol) solution with a mass concentration of 70% were mixed, cooled to 10°C, sulfuric acid (60.3 g, 0.4 mol) solution with a mass concentration of 65% was gradually added, stirred at 15°C for 2 hours, ice water was added, the organic layer was separated, washed with a KOH aqueous solution with a mass concentration of 5%, a colorless liquid was obtained, and then dried with anhydrous magnesium sulfate, i.e., a peroxide curing agent. The yield of the colorless liquid is 89.0%, and the purity by iodine titration is 99.3%.

[0043] Another peroxide curing agent is prepared by using tert-butyl hydroperoxide instead of tert-amyl hydroperoxide and adopting the synthesis steps of the above peroxide curing agent.

[0044] The present invention also provides a method for preparing a composite tread rubber elastomer, using the aforementioned component dosage ratio, the method comprising the following steps:

[0045] Step 1: Put styrene-butadiene rubber, silicone rubber compound, natural rubber and butadiene rubber into an internal mixer and plasticize them evenly; usually, plasticizing for about 1 to 5 minutes can make the various rubber materials evenly mixed;

[0046] Step 2: Add white carbon black, coupling agent and antioxidant, mix in an internal mixer (the temperature of the internal mixer gradually rises during this process), and discharge the rubber material when the temperature of the internal mixer reaches 130°C; a common method in this field is to add white carbon black, coupling agent and antioxidant into the internal mixer in batches to ensure uniform mixing;

[0047] Step 3: Add a vulcanizing agent and a co-vulcanizing agent to the rubber compound on an open mixing mill for vulcanization to obtain a composite tread rubber elastomer.

[0048] Preparing a silicone rubber compound before step 1 also belongs to the method for preparing the composite tread rubber elastomer described in the present invention.

[0049] Conventional vulcanization conditions in the art are a temperature of 155-170°C, a vulcanization pressure of 10-20 MPa, and a vulcanization time of 5-15 minutes. The mixed rubber obtained in step 1 and step 2 of the preparation method of the composite tread rubber elastomer can be vulcanized under conventional vulcanization conditions in the art to obtain the composite tread rubber elastomer. The embodiments and comparative examples of the present invention use vulcanization conditions of 160°C, 15 MPa, and a vulcanization time of 10 minutes.

[0050] Unlike CN105482200A, which directly mixes silicone rubber and styrene-butadiene rubber on an open mill, the present invention first uses a polythiol compound (i.e., a compatibilizer trimethylolpropane-tris(3-mercaptopropionic acid) ester) and silicone rubber to prepare a silicone rubber compound modified with an active thiol side group, and then blends it with styrene-butadiene rubber to produce a chemical bond at the interface between silicone rubber and styrene-butadiene rubber, reduce the size of the silicone rubber dispersed phase domain, and achieve two-step in-situ interface reaction capacity expansion. In order to solve the problem of uneven dispersion of fillers, a step-by-step dispersion technology is adopted. First, a white carbon black / silicone rubber raw rubber premixing method is used to match the viscosity of silicone rubber and styrene-butadiene rubber, solve the problem of the difficulty of the blending process caused by the low viscosity of silicone rubber raw rubber, increase the dispersion ratio of white carbon black in silicone rubber, and improve the "segregation" phenomenon of white carbon black in the two phases of silicone rubber and styrene-butadiene rubber, thereby improving the mechanical strength of the tread rubber.

[0051] Compared with the prior art, the present invention has at least the following beneficial effects:

[0052] (1) The present invention replaces part of the traditional styrene-butadiene rubber with silicone rubber, which has a positive driving force for the tire industry to replace imported raw materials and become self-sufficient;

[0053] (2) The present invention provides a tread rubber elastomer and a preparation method thereof, wherein the silicone rubber improves the wear resistance and aging resistance of the traditional tread rubber, and the tread rubber has a higher mechanical strength;

[0054] (3) The present invention provides a high-efficiency vulcanizing agent and its application in tread rubber, which solves the problem of difficult matching of vulcanization speeds when the tread rubber and the tire base rubber are co-vulcanized. DETAILED DESCRIPTION

[0055] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0056] Example 1

[0057] 100 parts of methyl vinyl silicone rubber (vinyl content 5%, molecular weight 600,000), 3 parts of hydroxy silicone oil (viscosity 40mPa.s), 35 parts of fumed silica, and 5 parts of trimethylolpropane-tris (3-mercaptopropionic acid) ester were kneaded into a mass in a kneader, and then vacuumed for 2 hours (vacuum -0.08MPa, temperature 120℃). The kneaded silicone rubber compound was cooled to room temperature, and the silicone rubber compound Mooney viscosity was 30 (1+4) 100℃.

[0058] 100 parts of solution polymerized styrene-butadiene rubber, 20 parts of silicone rubber compound, 5 parts of natural rubber (No. 1 standard rubber), and 5 parts of butadiene rubber (BR9000) were put into an internal mixer for plastication for 1 minute, and 20 parts of fumed silica, 45 parts of precipitated silica, 5 parts of coupling agent bis-[γ-(triethoxysilyl)propyl] tetrasulfide, 1.5 parts of antioxidant N-isopropyl-N'-phenyl-p-phenylenediamine, and 1.5 parts of antioxidant 2,2,4-trimethyl-1,2-dihydroquinoline polymer were added in batches and mixed together in an internal mixer. When the temperature of the internal mixer reaches 130°C, the rubber is discharged, and then the sheet is cooled on an open mixer to obtain a tread rubber compound.

[0059] Finally, 2.5 parts of a co-vulcanizing agent trimethylolpropane trimethacrylate and 3 parts of a peroxide vulcanizing agent 1,1-di(tert-amylperoxy)-3,5-dimethylcyclohexane represented by formula (1) were added on an open mill to obtain a tread rubber elastomer.

[0060] Example 2

[0061] The tread rubber elastomer was prepared using the process conditions of Example 1, except that the amount of trimethylolpropane-tris(3-mercaptopropionic acid) ester in Example 1 was adjusted to 2 parts. The Mooney viscosity of the silicone rubber compound was 35(1+4) at 100°C.

[0062] Example 3

[0063] The tread rubber elastomer was prepared using the process conditions of Example 1, except that the amount of the silicone rubber compound of Example 1 was adjusted to 30 parts.

[0064] Example 4

[0065] The tread rubber elastomer was prepared using the process conditions of Example 1, except that the coupling agent in Example 1 was adjusted to 3 parts of vinyl triethoxysilane.

[0066] Example 5

[0067] The process conditions of Example 1 were adopted to prepare the silicone rubber compound; the process conditions of Example 1 were adopted to prepare the tread rubber elastomer, except that the white carbon black added during the plasticating in the internal mixer of Example 1 was all adjusted to fumed white carbon black.

[0068] Example 6

[0069] The process conditions of Example 1 were adopted to prepare the silicone rubber compound; the process conditions of Example 1 were adopted to prepare the tread rubber elastomer, except that the white carbon black added during the plasticating in the internal mixer of Example 1 was all adjusted to precipitated white carbon black.

[0070] Example 7

[0071] The tread rubber elastomer was prepared using the process conditions of Example 1, except that the amounts of the co-vulcanizing agent and the vulcanizing agent of Example 1 were adjusted to: 2 parts of the co-vulcanizing agent trimethylolpropane trimethacrylate and 4 parts of the peroxide vulcanizing agent 1,1-di(tert-amylperoxy)-3,5-dimethylcyclohexane vulcanizing agent represented by formula (1).

[0072] Example 8

[0073] The tread rubber elastomer was prepared using the process conditions of Example 1, except that the vulcanizing agent in Example 1 was adjusted to 3 parts of 1,1-di(tert-butylperoxy)-3,5-dimethylcyclohexane.

[0074] The tread rubber elastomers prepared in Examples 1-8 were subjected to relevant mechanical property tests, and the testing method was as follows:

[0075] In order to obtain the positive vulcanization time T90 and the maximum torque MH, the vulcanization curve test was carried out at 160°C. The positive vulcanization time T90 can characterize the vulcanization molding time (vulcanization efficiency) of the rubber compound, and the maximum torque MH can characterize the crosslinking degree and crosslinking density of the rubber compound.

[0076] Shore A hardness: Use Shore A durometer to test hardness according to national standard GB / T531.1-2008.

[0077] Tensile strength: Prepare and test dumbbell-shaped samples according to the national standard GB / T528-2009.

[0078] Elongation at break: Prepare and test dumbbell-shaped samples according to the national standard GB / T528-2009.

[0079] Tear strength: Prepare and test dumbbell-shaped samples according to national standard GB / T529-2008.

[0080] Akron wear: Tested according to the national standard GB / T 1689-1998.

[0081] Peel strength: Tested according to the requirements of enterprise standard Q / WTCL 105-2021.

[0082] The test results of Examples 1-8 are shown in Table 1:

[0083] Table 1 Test results of tread rubber elastomer properties of Examples 1-8

[0084]

[0085] Note: 5'41" means 5 minutes and 41 seconds.

[0086] As can be seen from Table 1, Example 1 uses silicone rubber compound and styrene-butadiene rubber, natural rubber, and cis-1,4-dimethylbutyl rubber to mix, and uses the peroxide curing agent shown in formula (1) during the vulcanization process. The vulcanization time of the obtained tread rubber elastomer is within the range of 5 to 7 minutes of the vulcanization time of the tire base rubber, so the vulcanization speed of the tread rubber and the tire base rubber matches; the tread rubber elastomer has good mechanical properties (tensile strength, elongation at break, tear strength), and the Akron wear is low, indicating that the tread rubber elastomer has good wear resistance, and the peeling strength between the tire base rubber and the tread rubber is high, indicating that the tread rubber elastomer has good bonding performance with the tire base rubber, and the tread rubber is not easy to fall off. Because the compatibilizer is added to the silicone rubber compound, the compatibility of silicone rubber and styrene-butadiene rubber is good, and the macroscopic performance is high tensile strength and tear strength, and the Akron wear is low. After the tread rubber is treated at high temperature (100℃×72h), its tensile strength retention rate and elongation at break retention rate are both high, indicating that the tread rubber has good aging resistance.

[0087] Compared with Example 1, Example 2 reduces the amount of trimethylolpropane tris(3-mercaptopropionic acid) ester added as the compatibilizer, and the vulcanization time and the maximum torque have no difference, but the tensile strength and elongation are reduced.

[0088] In Example 3, compared with Example 1, the amount of silicone rubber compound added was increased to 30 parts, the tensile strength was reduced, but the elongation was increased.

[0089] In Example 4, compared with Example 1, the coupling agent is replaced with vinyl triethoxysilane, and the maximum torque MH is significantly increased, which proves that the crosslinking density and hardness are significantly improved.

[0090] Compared with Example 1, Example 5 uses fumed silica as all white carbon black, and the tensile strength and tear strength are significantly increased, the elongation at break is reduced, and the crosslinking density and hardness are improved.

[0091] Compared with Example 1, Example 6 uses precipitated silica, and the mechanical properties are reduced.

[0092] In Example 7, compared with Example 1, the addition amounts of the co-vulcanizing agent and the vulcanizing agent are changed.

[0093] In Example 8 compared with Example 1, the vulcanizing agent is 3 parts of 1,1-di(tert-butylperoxy)-3,5-dimethylcyclohexane, and its activity is slightly lower than that of 1,1-di(tert-amylperoxy)-3,5-dimethylcyclohexane. From the results, the vulcanization time is slightly longer, and the mechanical properties, aging resistance and wear resistance can still reach a good level, which has advantages over the prior art.

[0094] Although the various embodiments have different performances, compared with the prior art, the mechanical properties of the tread rubber are improved, the vulcanization speed matches that of the tire base rubber, and the tread rubber and the tire base rubber are better bonded.

[0095] Comparative Example 1

[0096] The difference between Comparative Example 1 and Example 1 is that the silicone rubber compound does not contain trimethylolpropane tris(3-mercaptopropionate) as a compatibilizer;

[0097] Comparative Example 2

[0098] The difference between Comparative Example 2 and Example 1 is that the vulcanizing agent is replaced by 3 parts of dicumyl peroxide;

[0099] Comparative Example 3

[0100] The difference between Comparative Example 3 and Example 1 is that the vulcanizing agent is replaced by 3 parts of 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane;

[0101] Comparative Example 4

[0102] The difference between Comparative Example 4 and Example 1 is that the vulcanizing agent is replaced by 3 parts of benzoyl peroxide;

[0103] Comparative Example 5

[0104] The difference between Comparative Example 5 and Example 1 is that no natural rubber and butadiene rubber are added.

[0105] Comparative Example 6

[0106] 100 parts of solution-polymerized styrene-butadiene rubber, 20 parts of methyl vinyl silicone rubber (vinyl content 5%, molecular weight 600,000), 5 parts of natural rubber, and 5 parts of butadiene rubber were put into an internal mixer for plastication for 1 minute, and 20 parts of fumed silica, 45 parts of precipitated silica, 5 parts of coupling agent bis-[γ-(triethoxysilyl)propyl] tetrasulfide, 1.5 parts of antioxidant N-isopropyl-N'-phenyl-p-phenylenediamine, and 1.5 parts of antioxidant 2,2,4-trimethyl-1,2-dihydroquinoline polymer were added in batches and mixed together in an internal mixer. When the temperature of the internal mixer reaches 130°C, the rubber is discharged, and then the sheet is cooled on an open mixer to obtain a mixed rubber for tread rubber.

[0107] Finally, 2.5 parts of a co-vulcanizing agent trimethylolpropane trimethacrylate and 3 parts of a peroxide vulcanizing agent 1,1-di(tert-amylperoxy)-3,5-dimethylcyclohexane represented by formula (1) were added on an open mill to obtain a tread rubber elastomer.

[0108] Comparative Example 7

[0109] The difference from Example 1 is that no silicone rubber compound is added.

[0110] The tread rubber properties of Comparative Examples 1-7 were obtained by the same testing method as in Example 1, as shown in Table 2.

[0111] Table 2 Tread rubber performance test results of Comparative Examples 1-7

[0112]

[0113]

[0114] From the results in Table 2, it can be seen that no compatibilizer is added to the silicone rubber compound of Comparative Example 1, resulting in poor compatibility between silicone rubber and styrene-butadiene rubber. Macroscopically, the tensile strength and tear strength are lower than those of Example 1. At the same time, the Akron abrasion is significantly increased and the aging resistance is reduced.

[0115] In Comparative Examples 2 and 3, the curing agents diisopropylbenzene peroxide and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane had a relatively long T90 time at 160°C, a slow curing efficiency, and low peel strength after co-curing with the tire base rubber. During the actual 240km / h high-speed tire running process, the tread rubber fell off.

[0116] Comparative Example 4 uses benzoyl peroxide as the vulcanizing agent, and the vulcanization speed is too fast, and there is also a problem of mismatch between the vulcanization speed of the tire base rubber and the short scorch time, which results in a short operating time of the rubber.

[0117] Compared with Example 1, Comparative Example 5 does not add natural rubber and butadiene rubber, and its tensile strength and tear strength are slightly reduced, and its vulcanization bonding fusion with the tire base rubber is slightly poor, and its peel strength is also significantly reduced.

[0118] In Comparative Example 6, the methyl vinyl silicone rubber was not prepared by the step-by-step method, and the methyl vinyl silicone rubber and styrene-butadiene rubber were directly mixed. From the results, it can be seen that the tensile strength, elongation at break, and tear strength are all reduced, and the Akron abrasion is increased, indicating that the mechanical properties and wear resistance are reduced.

[0119] Compared with Example 1, no silicone rubber compound was added in Comparative Example 7. As shown in Table 2, the tensile strength retention rate and elongation at break retention rate were significantly reduced. Therefore, adding silicone rubber compound to the composite tread rubber has a positive effect on improving the aging performance.

[0120] Although the present invention is described herein with reference to the illustrative embodiments of the present invention, the above embodiments are only preferred embodiments of the present invention, and the embodiments of the present invention are not limited to the above embodiments. It should be understood that those skilled in the art can design many other modifications and embodiments, which will fall within the scope and spirit of the principles disclosed in this application.

Claims

1. A composite tread rubber elastomer, It is characterized in that Made of the following components in parts by weight:

2. The composite tread rubber elastomer according to claim 1, It is characterized in that The silicone rubber compound is made of the following components in parts by weight:

3. The composite tread rubber elastomer according to claim 2, It is characterized in that The compatibilizer is trimethylolpropane-tris(3-mercaptopropionic acid) ester.

4. The composite tread rubber elastomer according to claim 3, It is characterized in that The molecular weight of the methyl vinyl silicone rubber is 350,000 to 650,000, and the vinyl content is 0.05% to 5%; the viscosity of the hydroxy silicone oil is 30 to 60 mPa.s.

5. The composite tread rubber elastomer according to claim 1, It is characterized in that The white carbon black is at least one of precipitated white carbon black and fumed white carbon black.

6. The composite tread rubber elastomer according to claim 1, It is characterized in that The natural rubber is No. 1 standard rubber, and the brand of butadiene rubber is BR9000.

7. The composite tread rubber elastomer according to claim 1, It is characterized in that The antioxidant is at least one of N-isopropyl-N'-phenyl-p-phenylenediamine and 2,2,4-trimethyl-1,2-dihydroquinoline polymer; the coupling agent is at least one of bis-[γ-(triethoxysilyl)propyl]tetrasulfide, γ-methacryloxypropyltrimethoxysilane and vinyltriethoxysilane.

8. The composite tread rubber elastomer according to claim 1, It is characterized in that The co-vulcanizing agent is at least one of trimethylolpropane trimethacrylate, triallyl isocyanurate and ethylene glycol diacrylate.

9. The composite tread rubber elastic body according to any one of claims 1 to 8, It is characterized in that The vulcanizing agent is a peroxide vulcanizing agent having the following structure: Where R is -C(CH 3 ) 3 or -CH 2 C(CH) 3 .

10. A method for preparing a composite tread rubber elastomer according to any one of claims 1 to 9, It is characterized in that The following steps are involved: Step 1: put methyl vinyl silicone rubber, white carbon black, hydroxy silicone oil and compatibilizer into a kneader for mixing, and after forming a mass, evacuate at 115-125° C. for at least 1 hour to obtain a silicone rubber compound; Step 2: Put styrene-butadiene rubber, silicone rubber compound, natural rubber and butadiene rubber into an internal mixer and plasticize them evenly; Step 3: Add white carbon black, coupling agent and antioxidant, mix in an internal mixer, and discharge the rubber when the temperature of the internal mixer reaches 130°C; Step 4: Add a vulcanizing agent and a vulcanizing aid into the rubber compound on an open mixing mill for vulcanization to obtain a composite tread rubber elastomer.