Anti-aging aerial cable and preparation method thereof
By using reinforcement additives and reinforcement fillers in overhead cables, a complex crosslinking network and a mesoporous structure of modified titanium oxide is formed, which solves the problem of degradation of adhesion at high temperatures and improves the aging resistance and service life of the cable.
Patent Information
- Application Number
- CN202410906853.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The adhesion of the semi-conductive shielding layer and the outer sheath layer under high temperature conditions has decreased, resulting in aging and affecting service life.
Using reinforcement additives and reinforcement fillers, a complex crosslinking network is formed through steam crosslinking and peroxide crosslinking agent, combining the mesoporous structure of modified titanium oxide and fluorine doping to enhance the aging resistance of the cable.
It improves the aging resistance of the outer sheath layer of the overhead cable, reduces light aging, improves the bonding performance between the semiconductor shielding layer and the outer sheath layer, and extends the service life of the cable.
Smart Images

Figure BDA0004932377090000101 
Figure BDA0004932377090000111
Abstract
Description
Technical Field
[0001] The invention relates to the field of overhead cables, and in particular to an aging-resistant overhead cable and a preparation method thereof. Background Art
[0002] Overhead cables have good insulation properties, electrical properties and mechanical strength. Taking into account safety, reliability, economy, easy maintenance and other factors, they are deeply loved by people. They have been widely used in 10kv distribution lines in urban and rural power grids and 35kv and below overhead power lines. Currently, common overhead cables usually include conductors, semi-conductive shielding layers and outer sheath layers.
[0003] However, during the wiring and tightening process of the overhead cable laid outdoors, the outer sheath layer of the overhead cable will be subjected to a large tensile force, and due to direct sunlight, the temperature of the overhead cable itself will rise rapidly, and the adhesion between the semi-conductive shielding layer and the outer sheath layer in the overhead cable will decrease, which will lead to the sheathing of the cable and the semi-conductive shielding layer falling off. Most of the outer sheath materials of overhead cables are cross-linked polyethylene. In order to improve the aging resistance of cross-linked polyethylene, titanium dioxide is usually added as an antioxidant. However, titanium dioxide has a wide bandgap, which means that it can only absorb sunlight with a shorter wavelength. As a result, in the long-term use process, direct sunlight will still cause the outer sheath layer of the overhead cable to age, thereby affecting the use of the overhead cable. Summary of the invention
[0004] The purpose of the present invention is to provide an aging-resistant overhead cable and a preparation method thereof, which solves the problem of decreased adhesion between the semi-conductive shielding layer and the outer sheath layer of the existing overhead cable under high temperature conditions, and at the same time has good aging resistance;
[0005] The object of the present invention can be achieved by the following technical solution: an aging-resistant overhead cable, which comprises, from inside to outside, a conductor, a semi-conductive shielding layer and an outer sheath layer;
[0006] A method for preparing an aging-resistant overhead cable comprises the following steps: Step S1: weighing the following raw materials in parts by weight: 80-90 parts of low-density polyethylene, 1-3 parts of a peroxide cross-linking agent, 0.8-1 parts of a lubricant, 8-10 parts of a reinforcing aid and 10-12 parts of a reinforcing filler, mixing the low-density polyethylene, the peroxide cross-linking agent, the lubricant, the reinforcing aid and the reinforcing filler and adding them to a twin-screw extruder, extruding and granulating, and obtaining an outer sheath layer raw material;
[0007] Step S2: passing the aluminum alloy rod into a wire drawing machine, drawing, annealing, and twisting the wire to obtain a conductor, and sequentially extruding the semi-conductive shielding layer material and the outer sheath layer material onto the conductor through double-layer co-extrusion, and steam cross-linking to obtain an aging-resistant overhead cable;
[0008] The reinforcing aid is prepared by the following steps:
[0009] Step A1: Mix cyanuric chloride and acetone, stir at a stirring rate of 300-400 rpm, add 7-hydroxy-4-methylcoumarin and N,N-dimethylacetamide, adjust the pH value to 6, react for 2-3 hours, then heat to 70° C., add 3-aminopropyltrimethoxysilane, adjust the pH value to 6, and react for 2-3 hours to obtain intermediate 1;
[0010] The dosage ratio of cyanuric chloride, 7-hydroxy-4-methylcoumarin, 3-aminopropyltrimethoxysilane, acetone and N,N-dimethylacetamide is 0.01-0.012 mol: 0.02-0.024 mol: 0.01-0.012 mol: 80-100 mL: 60-80 mL;
[0011] During the reaction, at room temperature, the chlorine in cyanuric chloride reacts with the hydroxyl group in 7-hydroxy-4-methylcoumarin to undergo a substitution reaction, and then at 70°C, the chlorine in cyanuric chloride reacts with the amino group in 3-aminopropyltrimethoxysilane to produce intermediate 1.
[0012] Step A2: Boric acid, tetraethyl orthosilicate, intermediate 1 and anhydrous ethanol are mixed, and the mixture is reacted for 15-20 minutes at a stirring rate of 180-240 rpm and a temperature of 80° C., and then tetramethyldivinyldisiloxane is added and the reaction is continued for 2-3 hours to obtain a reinforcing agent;
[0013] The amount ratio of boric acid, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, intermediate 1 and tetramethyldivinyldisiloxane is 0.1 mol: 0.18-0.2 mol: 0.1-0.12 mol: 0.08-0.1 mol;
[0014] During the reaction, in anhydrous ethanol, under acidic conditions, hydrolysis and condensation occur between boric acid and ethyl orthosilicate and between the silyl methoxy groups in the intermediate 1 to form silicon-oxygen-boron bonds, and then tetramethyldivinyldisiloxane is added to continue the reaction, and double bonds are introduced to obtain a reinforcing agent.
[0015] The reinforcing filler is prepared by the following steps:
[0016] Step B1: 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and N,N-dimethylacetamide were mixed, and anhydrous potassium carbonate was added under nitrogen protection at a stirring rate of 300-400 rpm and a temperature of 60°C, and the mixture was stirred for 32 hours to obtain intermediate a. Intermediate a, zinc acetate dihydrate and n-pentanol were mixed, and bicyclic amidine was added under nitrogen protection at a stirring rate of 300-400 rpm and a temperature of 140°C, and the mixture was stirred for 24 hours to obtain intermediate b;
[0017] The ratio of 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and anhydrous potassium carbonate is 0.01-0.012 mol: 0.01-0.012 mol: 3.5-4 g, and the ratio of intermediate a, zinc acetate dihydrate, n-pentanol and bicyclic amidine is 0.02-0.022 mol: 0.12-0.15 g: 15-18 mL: 1 mL;
[0018] During the reaction, under the condition of anhydrous potassium carbonate as an acid-binding agent, the hydroxyl group in 7-hydroxycoumarin-3-carboxylic acid reacts with the nitro group in 4-nitrophthalonitrile to form a carbon-oxygen-carbon ether bond to obtain intermediate a, and then in n-pentanol, under the catalysis of bicyclic amidine, intermediate a reacts with zinc acetate dihydrate to form a phthalocyanine structure to obtain intermediate b;
[0019] Step B2: cetyltrimethylammonium bromide, tetrabutyl titanate and anhydrous ethanol are mixed, stirred at a stirring rate of 250-300 rpm, and ammonium fluoride and deionized water are added at room temperature, stirred for 2-3 hours, heated to 120° C., reacted for 4-5 hours, centrifuged, dried, ground, and calcined at 500° C. for 4 hours to obtain modified titanium oxide;
[0020] The dosage ratio of hexadecyltrimethylammonium bromide, tetrabutyl titanate, anhydrous ethanol, ammonium fluoride and deionized water is 2.8-3g:8-10g:40-50mL:0.0008-0.001mol:8-10mL;
[0021] During the reaction, fluorine-doped modified titanium oxide with a mesoporous structure was prepared by a hydrothermal method using hexadecyltrimethylammonium bromide as a template, tetrabutyl titanate as a titanium source, and ammonium fluoride as a fluorine source.
[0022] Step B3: Mix the modified titanium oxide and anhydrous ethanol, stir at a stirring rate of 300-400 rpm and a temperature of 80° C., add methacryloxypropyltrimethoxysilane and deionized water, react for 2-3 hours, then add the intermediate b, and continue to react for 24 hours to obtain a reinforcing filler;
[0023] The usage ratio of modified titanium oxide, methacryloxypropyltrimethoxysilane, intermediate b, anhydrous ethanol and deionized water is 3-3.5 g: 0.8-1 mL: 0.001-0.0012 mol: 50-60 mL: 3-5 mL;
[0024] During the reaction, the silicon ethoxy group in the methacryloxypropyltrimethoxysilane is hydrolyzed and grafted onto the modified titanium oxide, and then the intermediate b is added, and the carboxyl group in the intermediate b is combined with the modified titanium oxide to obtain a reinforcing filler;
[0025] Beneficial effects of the invention: The invention relates to an aging-resistant overhead cable and a preparation method thereof, which solves the problem of decreased adhesion between the semi-conductive shielding layer and the outer sheath layer of the existing overhead cable under high temperature conditions, and at the same time has good aging resistance; reinforcing additives and reinforcing fillers are added to the raw materials of the outer sheath layer of the overhead cable, and since the reinforcing additives and the reinforcing fillers both contain unsaturated double bonds, under the action of the high temperature of steam crosslinking and the peroxide crosslinking agent, these double bonds are grafted into low-density polyethylene to form a complex crosslinking network, and since the reinforcing additives contain a large number of silicon-oxygen-boron groups, they can play a synergistic role with the crosslinking network, so that the outer sheath layer of the overhead cable has good aging resistance, and since the reinforcing additives and the reinforcing fillers both contain coumarin groups, coumarin The groups recombine with each other to consume energy under light, thereby reducing the aging of the outer sheath caused by light. Due to the presence of epoxy groups in the reinforcing additive, the bonding performance between the semi-conductive shielding layer and the outer sheath layer is improved, avoiding the degradation of bonding performance caused by high temperature. Since the reinforcing filler is made of modified titanium oxide as the matrix, the mesoporous structure and fluorine doping of the modified titanium oxide make it have better ultraviolet absorption ability, and the presence of the mesoporous structure also enables it to combine with more intermediates b. Under light conditions, the phthalocyanine structure in the intermediate b absorbs photons and is excited to produce free electrons. Then the excited intermediate b injects electrons into the conduction band of titanium oxide, thereby expanding the range of the excitation wavelength of titanium oxide, allowing it to repeatedly absorb visible light, thereby improving the aging resistance of the outer sheath layer of the overhead cable. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Embodiment 1 An aging-resistant overhead cable comprises, from inside to outside, a conductor, a semi-conductive shielding layer and an outer sheath layer;
[0028] A method for preparing an aging-resistant overhead cable comprises the following steps: Step S1: weighing the following raw materials in parts by weight: 80 parts of commercially available AT6101 low-density polyethylene, 1 part of di-tert-butyl peroxide crosslinking agent, 0.8 parts of commercially available YBS-S-8600 strontium platinum lubricant, 8 parts of reinforcing aids and 10 parts of reinforcing fillers, mixing the low-density polyethylene, the peroxide crosslinking agent, the lubricant, the reinforcing aid and the reinforcing filler and adding them to a twin-screw extruder, extruding and granulating, and obtaining the raw material for the outer sheath layer;
[0029] Step S2: passing the aluminum alloy rod into a wire drawing machine, drawing, annealing, and twisting the wire to obtain a conductor, and sequentially extruding the commercially available Haijiang V6110M semi-conductive shielding layer material and outer sheath layer material onto the conductor through double-layer co-extrusion, and steam cross-linking to obtain an aging-resistant overhead cable;
[0030] The reinforcing aid is prepared by the following steps:
[0031] Step A1: cyanuric chloride and acetone were mixed, stirred at a stirring rate of 300 rpm, and 7-hydroxy-4-methylcoumarin and N,N-dimethylacetamide were added, and the pH value was adjusted to 6, and the reaction was carried out for 2 hours. The temperature was then raised to 70° C., 3-aminopropyltrimethoxysilane was added, and the pH value was adjusted to 6, and the reaction was carried out for 2 hours to obtain intermediate 1;
[0032] The amount ratio of cyanuric chloride, 7-hydroxy-4-methylcoumarin, 3-aminopropyltrimethoxysilane, acetone and N,N-dimethylacetamide is 0.01mol:0.02mol:0.01mol:80mL:60mL;
[0033] Step A2: Boric acid, tetraethyl orthosilicate, intermediate 1 and anhydrous ethanol were mixed, and the mixture was reacted for 15 min at a stirring rate of 180 rpm and a temperature of 80° C., and then tetramethyldivinyldisiloxane was added and the reaction was continued for 2 h to obtain a reinforcing agent;
[0034] The amount ratio of boric acid, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, intermediate 1 and tetramethyldivinyldisiloxane is 0.1 mol: 0.18 mol: 0.1 mol: 0.08 mol;
[0035] The reinforcing filler is prepared by the following steps:
[0036] Step B1: 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and N,N-dimethylacetamide were mixed, and anhydrous potassium carbonate was added under nitrogen protection at a stirring rate of 300 rpm and a temperature of 60°C, and the mixture was stirred for 32 hours to obtain intermediate a. Intermediate a, zinc acetate dihydrate and n-pentanol were mixed, and bicyclic amidine was added under nitrogen protection at a stirring rate of 300 rpm and a temperature of 140°C, and the mixture was stirred for 24 hours to obtain intermediate b.
[0037] The ratio of 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and anhydrous potassium carbonate is 0.01 mol: 0.01 mol: 3.5 g, and the ratio of intermediate a, zinc acetate dihydrate, n-pentanol and bicyclic amidine is 0.02 mol: 0.12 g: 15 mL: 1 mL;
[0038] Step B2: Hexadecyltrimethylammonium bromide, tetrabutyl titanate and anhydrous ethanol were mixed, stirred at a stirring rate of 250 rpm, and ammonium fluoride and deionized water were added, stirred for 2 hours, heated to 120°C, reacted for 4 hours, centrifuged, dried, ground, and calcined at 500°C for 4 hours to obtain modified titanium oxide;
[0039] The dosage ratio of hexadecyltrimethylammonium bromide, tetrabutyl titanate, anhydrous ethanol, ammonium fluoride and deionized water is 2.8g:8g:40mL:0.0008mol:8mL;
[0040] Step B3: Modified titanium oxide and anhydrous ethanol were mixed, and methacryloxypropyltrimethoxysilane and deionized water were added under stirring conditions of a stirring rate of 300 rpm and a temperature of 80° C. The mixture was reacted for 2 h, and then intermediate b was added and the reaction was continued for 24 h to obtain a reinforcing filler;
[0041] The usage ratio of modified titanium oxide, methacryloxypropyltrimethoxysilane, intermediate b, anhydrous ethanol and deionized water is 3g:0.8mL:0.001mol:50mL:3mL.
[0042] Embodiment 1 An aging-resistant overhead cable comprises, from inside to outside, a conductor, a semi-conductive shielding layer and an outer sheath layer;
[0043] A method for preparing an aging-resistant overhead cable comprises the following steps: Step S1: weighing the following raw materials in parts by weight: 80 parts of commercially available AT6101 low-density polyethylene, 1 part of di-tert-butyl peroxide crosslinking agent, 1 part of commercially available YBS-S-8600 strontium platinum lubricant, 8 parts of reinforcing aids and 10 parts of reinforcing fillers, mixing the low-density polyethylene, the peroxide crosslinking agent, the lubricant, the reinforcing aid and the reinforcing filler and adding them to a twin-screw extruder, extruding and granulating, and obtaining the raw material for the outer sheath layer;
[0044] Step S2: passing the aluminum alloy rod into a wire drawing machine, drawing, annealing, and twisting the wire to obtain a conductor, and sequentially extruding the commercially available Haijiang V6110M semi-conductive shielding layer material and outer sheath layer material onto the conductor through double-layer co-extrusion, and steam cross-linking to obtain an aging-resistant overhead cable;
[0045] The reinforcing aid is prepared by the following steps:
[0046] Step A1: cyanuric chloride and acetone were mixed, stirred at a stirring rate of 300 rpm, and 7-hydroxy-4-methylcoumarin and N,N-dimethylacetamide were added, and the pH value was adjusted to 6, and the reaction was carried out for 3 hours. The temperature was then raised to 70° C., 3-aminopropyltrimethoxysilane was added, and the pH value was adjusted to 6, and the reaction was carried out for 2 hours to obtain intermediate 1;
[0047] The amount ratio of cyanuric chloride, 7-hydroxy-4-methylcoumarin, 3-aminopropyltrimethoxysilane, acetone and N,N-dimethylacetamide is 0.012mol:0.02mol:0.012mol:80mL:80mL;
[0048] Step A2: Boric acid, ethyl orthosilicate, intermediate 1 and anhydrous ethanol were mixed, and the mixture was reacted for 20 min at a stirring rate of 180 rpm and a temperature of 80° C., and then tetramethyldivinyldisiloxane was added and the reaction was continued for 2 h to obtain a reinforcing agent;
[0049] The amount ratio of boric acid, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, intermediate 1 and tetramethyldivinyldisiloxane is 0.1 mol: 0.2 mol: 0.1 mol: 0.1 mol;
[0050] The reinforcing filler is prepared by the following steps:
[0051] Step B1: 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and N,N-dimethylacetamide were mixed, and anhydrous potassium carbonate was added under nitrogen protection at a stirring rate of 300 rpm and a temperature of 60°C, and the mixture was stirred for 32 hours to obtain intermediate a. Intermediate a, zinc acetate dihydrate and n-pentanol were mixed, and bicyclic amidine was added under nitrogen protection at a stirring rate of 400 rpm and a temperature of 140°C, and the mixture was stirred for 24 hours to obtain intermediate b.
[0052] The ratio of 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and anhydrous potassium carbonate is 0.01 mol: 0.01 mol: 4 g, and the ratio of intermediate a, zinc acetate dihydrate, n-pentanol and bicyclic amidine is 0.022 mol: -0.15 g: 15 mL: 1 mL;
[0053] Step B2: Hexadecyltrimethylammonium bromide, tetrabutyl titanate and anhydrous ethanol were mixed, stirred at a stirring rate of 250 rpm, and ammonium fluoride and deionized water were added, stirred for 3 hours, heated to 120°C, reacted for 4 hours, centrifuged, dried, ground, and calcined at 500°C for 4 hours to obtain modified titanium oxide;
[0054] The dosage ratio of hexadecyltrimethylammonium bromide, tetrabutyl titanate, anhydrous ethanol, ammonium fluoride and deionized water is 2.8g:10g:50mL:0.0008mol:10mL;
[0055] Step B3: Mix the modified titanium oxide and anhydrous ethanol, stir at a stirring rate of 300 rpm and a temperature of 80° C., add methacryloxypropyltrimethoxysilane and deionized water, react for 3 h, then add intermediate b, and continue to react for 24 h to obtain a reinforcing filler;
[0056] The dosage ratio of modified titanium oxide, methacryloxypropyltrimethoxysilane, intermediate b, anhydrous ethanol and deionized water is 3:1 mL:0.0012 mol:50 mL:5 mL.
[0057] Embodiment 3 An aging-resistant overhead cable comprises, from inside to outside, a conductor, a semi-conductive shielding layer and an outer sheath layer;
[0058] A method for preparing an aging-resistant overhead cable comprises the following steps: Step S1: weighing the following raw materials in parts by weight: 90 parts of commercially available AT6101 low-density polyethylene, 3 parts of di-tert-butyl peroxide crosslinking agent, 1 part of commercially available YBS-S-8600 strontium platinum lubricant, 10 parts of reinforcing aids and 12 parts of reinforcing fillers, mixing the low-density polyethylene, the peroxide crosslinking agent, the lubricant, the reinforcing aid and the reinforcing filler and adding them to a twin-screw extruder, extruding and granulating, and obtaining the raw material for the outer sheath layer;
[0059] Step S2: passing the aluminum alloy rod into a wire drawing machine, drawing, annealing, and twisting the wire to obtain a conductor, and sequentially extruding the commercially available Haijiang V6110M semi-conductive shielding layer material and outer sheath layer material onto the conductor through double-layer co-extrusion, and steam cross-linking to obtain an aging-resistant overhead cable;
[0060] The reinforcing aid is prepared by the following steps:
[0061] Step A1: cyanuric chloride and acetone were mixed, stirred at a stirring rate of 400 rpm, and 7-hydroxy-4-methylcoumarin and N,N-dimethylacetamide were added, and the pH value was adjusted to 6, and the reaction was carried out for 3 hours. The temperature was then raised to 70° C., 3-aminopropyltrimethoxysilane was added, and the pH value was adjusted to 6, and the reaction was carried out for 3 hours to obtain intermediate 1;
[0062] The amount ratio of cyanuric chloride, 7-hydroxy-4-methylcoumarin, 3-aminopropyltrimethoxysilane, acetone and N,N-dimethylacetamide is 0.012 mol: 0.024 mol: 0.012 mol: 100 mL: 80 mL;
[0063] Step A2: Boric acid, tetraethyl orthosilicate, intermediate 1 and anhydrous ethanol were mixed, and the mixture was reacted for 20 min at a stirring rate of 240 rpm and a temperature of 80° C., and then tetramethyldivinyldisiloxane was added and the reaction was continued for 3 h to obtain a reinforcing agent;
[0064] The amount ratio of boric acid, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, intermediate 1 and tetramethyldivinyldisiloxane is 0.1 mol: 0.2 mol: 0.12 mol: 0.1 mol;
[0065] The reinforcing filler is prepared by the following steps:
[0066] Step B1: 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and N,N-dimethylacetamide were mixed, and anhydrous potassium carbonate was added under nitrogen protection at a stirring rate of 400 rpm and a temperature of 60°C, and the mixture was stirred for 32 hours to obtain intermediate a. Intermediate a, zinc acetate dihydrate and n-pentanol were mixed, and bicyclic amidine was added under nitrogen protection at a stirring rate of 400 rpm and a temperature of 140°C, and the mixture was stirred for 24 hours to obtain intermediate b.
[0067] The ratio of 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and anhydrous potassium carbonate is 0.012 mol: 0.012 mol: 4 g, and the ratio of intermediate a, zinc acetate dihydrate, n-pentanol and bicyclic amidine is 0.022 mol: 0.15 g: 18 mL: 1 mL;
[0068] Step B2: Hexadecyltrimethylammonium bromide, tetrabutyl titanate and anhydrous ethanol were mixed, stirred at a stirring rate of 300 rpm, and ammonium fluoride and deionized water were added at room temperature, stirred for 3 hours, heated to 120°C, reacted for 5 hours, centrifuged, dried, ground, and calcined at 500°C for 4 hours to obtain modified titanium oxide;
[0069] The dosage ratio of hexadecyltrimethylammonium bromide, tetrabutyl titanate, anhydrous ethanol, ammonium fluoride and deionized water is -3g:10g:50mL:0.001mol:10mL;
[0070] Step B3: Mix the modified titanium oxide and anhydrous ethanol, stir at a stirring rate of 400 rpm and a temperature of 80° C., add methacryloxypropyltrimethoxysilane and deionized water, react for 3 h, then add intermediate b, and continue to react for 24 h to obtain a reinforcing filler;
[0071] The dosage ratio of modified titanium oxide, methacryloxypropyltrimethoxysilane, intermediate b, anhydrous ethanol and deionized water is 3.5 g: 1 mL: 0.0012 mol: 60 mL: 5 mL.
[0072] Comparative Example 1 Compared with Example 3, this comparative example is characterized in that 3-(2,3-epoxypropoxy)propyltrimethoxysilane in the preparation process of the reinforcing auxiliary agent in Example 3 is replaced by butyltrimethoxysilane, and the other steps are the same.
[0073] Comparative Example 2 Compared with Example 3, this comparative example is characterized in that 7-hydroxy-4-methylcoumarin in the preparation process of the reinforcing auxiliary agent in Example 3 is replaced by phenol, and the other steps are the same.
[0074] Comparative Example 3 Compared with Example 3, this comparative example is characterized in that the intermediate b in the preparation process of the reinforcing filler in Example 3 is removed, and the other steps are the same.
[0075] Comparative Example 4 Compared with Example 3, this comparative example removes ammonium fluoride during the preparation of the reinforcing filler in Example 3, and the other steps are the same.
[0076] Take an aging-resistant overhead cable prepared in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4, refer to GB / T 14049-2008, cut the aging-resistant overhead cable into samples with a length of 300 mm, place the samples at room temperature and 50°C for 4 hours, and then test the insulation adhesion. The outer sheath layer of the aging-resistant overhead cable is peeled off and prepared as a sample. Refer to GB / T 1040.2-2022, at room temperature and a tensile rate of 50 mm / min, the tensile performance test is performed on it, the sample is placed in a solar radiation aging test box, the aging time is 27 days, and the mechanical properties after aging are tested. The test results are as follows:
[0077]
[0078]
[0079] It can be seen from the test results in the table shown that when Example 1, Example 2 and Example 3 are compared with Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4, Comparative Example 1 replaces 3-(2,3-epoxypropoxy)propyltrimethoxysilane with butyltrimethoxysilane in the preparation process of the reinforcing auxiliary agent in Example 3. Due to the lack of epoxy groups, its adhesion performance under high temperature conditions is greatly reduced. Comparative Example 2 replaces 7-hydroxy-4-methylcoumarin with phenol in the preparation process of the reinforcing auxiliary agent in Example 3. Due to the lack of coumarin groups, its aging resistance is reduced. Comparative Example 3 removes intermediate b in the preparation process of the reinforcing filler in Example 3. Due to the lack of phthalocyanine structure, its aging resistance is reduced. Comparative Example 4 removes ammonium fluoride in the preparation process of the reinforcing filler in Example 3. Due to the lack of fluorine doping, its aging resistance is reduced.
[0080] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0081] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing an aging-resistant overhead cable, characterized in that: The method comprises the following steps: Step S1: weighing the following raw materials in parts by weight: 80-90 parts of low-density polyethylene, 1-3 parts of a peroxide crosslinking agent, 0.8-1 parts of a lubricant, 8-10 parts of a reinforcing aid and 10-12 parts of a reinforcing filler, mixing the low-density polyethylene, the peroxide crosslinking agent, the lubricant, the reinforcing aid and the reinforcing filler and adding them to a twin-screw extruder, extruding and granulating, and obtaining a raw material for an outer sheath layer; Step S2: passing the aluminum alloy rod into a wire drawing machine, drawing, annealing, and twisting the wire to obtain a conductor, and sequentially extruding the semi-conductive shielding layer material and the outer sheath layer material onto the conductor through double-layer co-extrusion, and steam cross-linking to obtain an aging-resistant overhead cable.
2. The method for preparing an aging-resistant overhead cable according to claim 1, characterized in that: The reinforcing aid is prepared by the following steps: Step A1: Mix cyanuric chloride and acetone, stir at a stirring rate of 300-400 rpm, add 7-hydroxy-4-methylcoumarin and N,N-dimethylacetamide, adjust the pH value to 6, react for 2-3 hours, then heat to 70° C., add 3-aminopropyltrimethoxysilane, adjust the pH value to 6, and react for 2-3 hours to obtain intermediate 1; Step A2: Boric acid, ethyl orthosilicate, intermediate 1 and anhydrous ethanol are mixed, and the mixture is reacted for 15-20 minutes at a stirring rate of 180-240 rpm and a temperature of 80° C. Then tetramethyldivinyldisiloxane is added and the reaction is continued for 2-3 hours to obtain a reinforcing agent.
3. The method for preparing an aging-resistant overhead cable according to claim 2, characterized in that: In step A1, the usage ratio of cyanuric chloride, 7-hydroxy-4-methylcoumarin, 3-aminopropyltrimethoxysilane, acetone and N,N-dimethylacetamide is 0.01-0.012 mol: 0.02-0.024 mol: 0.01-0.012 mol: 80-100 mL: 60-80 mL.
4. The method for preparing an aging-resistant overhead cable according to claim 2, characterized in that: In step A2, the amount ratio of boric acid, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, intermediate 1 and tetramethyldivinyldisiloxane is 0.1 mol: 0.18-0.2 mol: 0.1-0.12 mol: 0.08-0.1 mol.
5. The method for preparing an aging-resistant overhead cable according to claim 1, characterized in that: The reinforcing filler is prepared by the following steps: Step B1: 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and N,N-dimethylacetamide were mixed, and anhydrous potassium carbonate was added under nitrogen protection at a stirring rate of 300-400 rpm and a temperature of 60°C, and the mixture was stirred for 32 hours to obtain intermediate a. Intermediate a, zinc acetate dihydrate and n-pentanol were mixed, and bicyclic amidine was added under nitrogen protection at a stirring rate of 300-400 rpm and a temperature of 140°C, and the mixture was stirred for 24 hours to obtain intermediate b; Step B2: mix hexadecyltrimethylammonium bromide, tetrabutyl titanate and anhydrous ethanol, stir and add ammonium fluoride and deionized water at a stirring rate of 250-300 rpm at room temperature, stir for 2-3 hours, heat to 120°C, react for 4-5 hours, centrifuge, dry, grind, and calcine at 500°C for 4 hours to obtain modified titanium oxide. Step B3: Mix the modified titanium oxide and anhydrous ethanol, stir and add methacryloxypropyltrimethoxysilane and deionized water at a stirring rate of 300-400 rpm and a temperature of 80°C, react for 2-3 hours, then add intermediate b and continue to react for 24 hours to obtain a reinforcing filler.
6. The method for preparing an aging-resistant overhead cable according to claim 5, characterized in that: In step B1, the ratio of 7-hydroxycoumarin-3-carboxylic acid, 4-nitrophthalonitrile and anhydrous potassium carbonate is 0.01-0.012 mol: 0.01-0.012 mol: 3.5-4 g, and the ratio of intermediate a, zinc acetate dihydrate, n-pentanol and bicyclic amidine is 0.02-0.022 mol: 0.12-0.15 g: 15-18 mL: 1 mL.
7. The method for preparing an aging-resistant overhead cable according to claim 5, characterized in that: In step B2, the dosage ratio of hexadecyltrimethylammonium bromide, tetrabutyl titanate, anhydrous ethanol, ammonium fluoride and deionized water is 2.8-3 g: 8-10 g: 40-50 mL: 0.0008-0.001 mol: 8-10 mL.
8. The method for preparing an aging-resistant overhead cable according to claim 5, characterized in that: In step B3: the usage ratio of modified titanium oxide, methacryloxypropyltrimethoxysilane, intermediate b, anhydrous ethanol and deionized water is 3-3.5 g: 0.8-1 mL: 0.001-0.0012 mol: 50-60 mL: 3-5 mL.
9. An aging-resistant overhead cable, characterized in that: From the inside to the outside, there are a conductor, a semi-conductive shielding layer and an outer sheath layer, and they are prepared according to any one of the preparation methods described in claims 1-8.
Citation Information
Patent Citations
Preparation of fluorine and carbon co-doped nano-titanium dioxide visible light photocatalyst
CN101862664A
Fluorinated coumarin-phthalocyanine conjugate and preparation method and application thereof
CN103435624A
Triazinyl coumarin type fluorescent whitening agent, and preparation method and application thereof
CN110950851A
Color-adjustable environment-friendly water-based ink and preparation method thereof
CN112322106A
Antibacterial polyethylene film and preparation method thereof
CN116376079A
Cited By
Anti-aging aerial cable
CN120464093A
Anti-aging resin material and preparation method thereof
CN121108645A