Fluororubber sealing material resistant to high temperature, high pressure and intense radiation and preparation method thereof
Fluororubber materials prepared through specific proportions and processes have solved the problem of insufficient performance under high temperature, high pressure and strong radiation environments, achieving excellent mechanical properties and long-term stable operation, and are suitable for sealing materials in nuclear island equipment.
Patent Information
- Application Number
- CN202411125426.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
AI Technical Summary
Existing fluororubber materials do not perform well under high temperature, high pressure and strong radiation environments, making it difficult to provide long-term stable operation.
High-temperature, high-pressure, and high-radiation fluororubber sealing materials are prepared by using a specific ratio of fluororubber base polymer, crosslinking agent, activator, anti-aging agent, antioxidant, heat stabilizer, softener, high-temperature stabilizing filler, high-pressure stabilizing filler, and radiation-resistant filler through plasticizing, mixing, vulcanization, molding, and secondary vulcanization.
The prepared fluororubber material exhibits excellent mechanical properties under high temperature, high pressure and strong radiation environments, meeting the technical requirements for nuclear island-level sealing and ensuring the long-term stable operation of the equipment.
Smart Images

Figure CN118879008A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fluororubber, in particular to a high-temperature, high-pressure and strong-radiation resistant fluororubber sealing material and a preparation method thereof. Background Art
[0002] Fluororubber, because of its fluorine atoms, has the characteristics of high temperature resistance, oil resistance and resistance to corrosion by various chemicals. Fluororubber sealing material refers to a synthetic polymer elastomer containing fluorine atoms on the carbon atoms of the main chain or side chain, that is, a sealing material made of fluorine rubber (Fluororubber or FKM). The existing fluorine rubber preparation materials are not easy to have excellent mechanical properties, and their adaptability to high temperature, high pressure and strong radiation environments is relatively general, and it is not easy to provide long-term stable operation guarantee. Summary of the invention
[0003] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a high temperature, high pressure and strong radiation resistant fluororubber sealing material and a preparation method thereof.
[0004] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a high temperature, high pressure and strong radiation resistant fluororubber sealing material, comprising the following raw materials in parts by weight: 100 parts of fluororubber base polymer, 3 to 6 parts of cross-linking agent, 0.5 to 2 parts of activator, 2 to 6 parts of antioxidant, 0.1 to 2 parts of antioxidant and heat stabilizer, 2 to 10 parts of softener, 10 to 30 parts of high temperature stable filler, 10 to 30 parts of high pressure stable filler, and 5 to 20 parts of radiation resistant filler.
[0005] Preferably, the base polymer of the fluororubber is formed by adding vinylidene fluoride (VE2) as the main monomer and hexafluoropropylene (HFP) as the comonomer, and adding a small amount of tetrafluoroethylene (TFE) to form the base polymer of the fluororubber, and the crosslinking agent is one or both of diisopropylbenzene peroxide (DCP) and di-tert-butyl peroxide (DTBP).
[0006] Preferably, the activator is one or more of the thiuram activators MBT, MBTS, MBS, DZ, and TMTD, and the antioxidant is one or more of N-cyclohexyl-N'-phenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, and N-(1,3-dimethyl)butyl-N'-phenyl-p-phenylenediamine.
[0007] Preferably, the antioxidant is one or more of the phenolic oxidants lrganox 1010, 1076, and BHT; the heat stabilizer is one or both of zinc oxide and magnesium oxide.
[0008] Preferably, the softener is fluorinated oil.
[0009] Preferably, the high temperature stable filler is one or more of graphene, N770, and N990.
[0010] Preferably, the high pressure stable filler is carbon fiber.
[0011] Preferably, the radiation-resistant filler is one or more of aluminum oxide, zirconium oxide, titanium oxide, and yttrium oxide.
[0012] A method for preparing a high temperature, high pressure and strong radiation resistant fluororubber sealing material comprises the following steps:
[0013] Step 1: Ingredients: weigh each raw material component according to the proportion;
[0014] Step 2: Plastication, raising the roller temperature of the open mill to 65±5°C and maintaining it, plasticating the base polymer of the fluororubber and producing sheets;
[0015] Step 3: Mixing: Put the plasticized fluororubber sheet and the pre-mixed various additives and fillers into an internal mixer for mixing. During this process, the temperature should be controlled between 120℃ and 140℃;
[0016] Step 4: refining, vulcanizing, discharging and parking, controlling the roller temperature at 65±5℃ and maintaining it, adding vulcanizing agent for vulcanization process, mixing with an eight-shaped knife, making triangle bags, thinning, discharging, and parking the mixed rubber;
[0017] Step 5: Molding: According to product requirements, the mixed rubber sheet is molded or extruded into a semi-finished product;
[0018] Step 6: Vulcanization: put the semi-finished rubber into the vulcanizer for vulcanization. The temperature of the vulcanizer is controlled at 180±5℃. The pressure and time are adjusted according to different products.
[0019] Step 7: Second stage vulcanization: put the product into a high temperature box for secondary vulcanization, step by step increase the temperature to 200°C, and maintain for 12 hours.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The high temperature, high pressure and strong radiation resistant fluororubber sealing material prepared by the present invention has excellent mechanical properties while taking into account high temperature, high pressure and strong radiation resistance, meets the technical requirements of nuclear island-level sealing for materials, and can provide strong guarantees for the long-term stable operation of generators, heat exchangers, pumps, valves, pipelines and accessories, containers, etc. inside and outside the nuclear island. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The present invention is a flow chart for preparing the high temperature, high pressure and strong radiation resistant fluororubber sealing material. DETAILED DESCRIPTION
[0023] See also Figure 1 The present invention provides a technical solution: a high temperature, high pressure and strong radiation resistant fluororubber sealing material, comprising the following raw materials in parts by weight: 100 parts of fluororubber base polymer, 3 to 6 parts of crosslinking agent, 0.5 to 2 parts of activator, 2 to 6 parts of antioxidant, 0.1 to 2 parts of antioxidant and heat stabilizer, 2 to 10 parts of softener, 10 to 30 parts of high temperature stable filler, 10 to 30 parts of high pressure stable filler, and 5 to 20 parts of radiation resistant filler;
[0024] The base polymer of fluororubber is formed by adding a small amount of tetrafluoroethylene (TFE) to form the base polymer of fluororubber, with vinylidene fluoride (VE2) as the main monomer and hexafluoropropylene (HFP) as the comonomer. The crosslinking agent is one or two of dicumyl peroxide (DCP) and di-tert-butyl peroxide (DTBP). The activator is one or more of thiuram activators MBT, MBTS, MBS, DZ, and TMTD. The antioxidant is one or more of N-cyclohexyl-N'-phenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, and N-(1,3-dimethyl)butyl-N'-phenyl-p-phenylenediamine. The antioxidant is a phenolic oxidant lrganox. One or more of 1010, 1076, and BHT; the heat stabilizer is one or both of zinc oxide and magnesium oxide; the softener is fluorinated oil; the high-temperature stable filler is one or more of graphene, N770, and N990; the high-pressure stable filler is carbon fiber; the radiation-resistant filler is one or more of aluminum oxide, zirconium oxide, titanium oxide, and yttrium oxide.
[0025] A method for preparing a high temperature, high pressure and strong radiation resistant fluororubber sealing material comprises the following steps:
[0026] Step 1: Ingredients: weigh each raw material component according to the proportion;
[0027] Step 2: Plastication, raising the roller temperature of the open mill to 65±5°C and maintaining it, plasticating the base polymer of the fluororubber and producing sheets;
[0028] Step 3: Mixing: Put the plasticized fluororubber sheet and the pre-mixed various additives and fillers into an internal mixer for mixing. During this process, the temperature should be controlled between 120℃ and 140℃;
[0029] Step 4: refining, vulcanizing, discharging and parking, controlling the roller temperature at 65±5℃ and maintaining it, adding vulcanizing agent for vulcanization process, mixing with an eight-shaped knife, making triangle bags, thinning, discharging, and parking the mixed rubber;
[0030] Step 5: Molding: According to product requirements, the mixed rubber sheet is molded or extruded into a semi-finished product;
[0031] Step 6: Vulcanization: put the semi-finished rubber into the vulcanizer for vulcanization. The temperature of the vulcanizer is controlled at 180±5℃. The pressure and time are adjusted according to different products.
[0032] Step 7: Second stage vulcanization: put the product into a high temperature box for secondary vulcanization, step by step increase the temperature to 200°C, and maintain for 12 hours.
[0033]
[0034] Table 2 Test results of radiation-resistant fluororubber materials for nuclear power
[0035]
[0036]
[0037] Note: *Test condition is 25% compression rate
[0038] After irradiation with a cumulative dose of 5x10'Gy and a dose rate of 200Gy, the results are shown in Table 2: after irradiation, the hardness of the fluororubber in the embodiment decreases by 12A at most, the compression permanent deformation is good, both within the standard range, the tensile strength decreases by 22% at most, the elongation at break increases by 29% at most, and decreases by 14%. The comprehensive performance of the rubber is good, and the elasticity is good. The rubber products made in the embodiment have good sealing function.
[0039] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technical changes and equivalent structural changes based on the present invention are still within the protection scope of any simple modification scheme made to the above embodiments based on the technical essence of the present invention.
Claims
1. A fluororubber sealing material resistant to high temperature, high pressure and strong radiation. It is characterized in that The invention comprises the following raw materials in parts by weight: 100 parts of a base polymer of fluororubber, 3 to 6 parts of a crosslinking agent, 0.5 to 2 parts of an activator, 2 to 6 parts of an antioxidant, 0.1 to 2 parts of an antioxidant and a heat stabilizer, 2 to 10 parts of a softener, 10 to 30 parts of a high-temperature stable filler, 10 to 30 parts of a high-pressure stable filler, and 5 to 20 parts of a radiation-resistant filler.
2. A high temperature, high pressure and strong radiation resistant fluororubber sealing material according to claim 1, Features: The base polymer of the fluororubber is formed by adding vinylidene fluoride (VE2) as the main monomer and hexafluoropropylene (HFP) as the comonomer, and adding a small amount of tetrafluoroethylene (TFE). The crosslinking agent is one or both of diisopropylbenzene peroxide (DCP) and di-tert-butyl peroxide (DTBP).
3. The high temperature, high pressure and strong radiation resistant fluororubber sealing material according to claim 1, Features: The activator is one or more of thiuram activators MBT, MBTS, MBS, DZ, and TMTD, and the antioxidant is one or more of N-cyclohexyl-N'-phenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, and N-(1,3-dimethyl)butyl-N'-phenyl-p-phenylenediamine.
4. The high temperature, high pressure and strong radiation resistant fluororubber sealing material according to claim 1, Features: The antioxidant is one or more of the phenolic oxidants lrganox 1010, 1076, and BHT; the heat stabilizer is one or two of zinc oxide and magnesium oxide.
5. The high temperature, high pressure and strong radiation resistant fluororubber sealing material according to claim 1, Features: The softener is fluorinated oil.
6. The high temperature, high pressure and strong radiation resistant fluororubber sealing material according to claim 1, Features: The high temperature stable filler is one or more of graphene, N770 and N990.
7. The high temperature, high pressure and strong radiation resistant fluororubber sealing material according to claim 1, Features: The high pressure stable filler is carbon fiber.
8. The high temperature, high pressure and strong radiation resistant fluororubber sealing material according to claim 1, Features: The radiation-resistant filler is one or more of aluminum oxide, zirconium oxide, titanium oxide and yttrium oxide.
9. A method for preparing a high temperature, high pressure and strong radiation resistant fluororubber sealing material according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Step 1: Ingredients: weigh each raw material component according to the proportion; Step 2: Plastication, raising the roller temperature of the open mill to 65±5°C and maintaining it, plasticating the base polymer of the fluororubber and producing sheets; Step 3: Mixing: Put the plasticized fluororubber sheet and the pre-mixed various additives and fillers into the internal mixer for mixing. During this process, the temperature should be controlled between 120℃ and 140℃; Step 4: refining, vulcanizing, discharging and parking, controlling the roller temperature at 65±5℃ and maintaining it, adding vulcanizing agent for vulcanization process, mixing with an eight-shaped knife, making triangle bags, thinning, discharging, and parking the mixed rubber; Step 5: Molding: According to product requirements, the mixed rubber sheet is molded or extruded into a semi-finished product; Step 6: Vulcanization: put the semi-finished rubber into the vulcanizer for vulcanization. The temperature of the vulcanizer is controlled at 180±5℃. The pressure and time are adjusted according to different products. Step 7: Second stage vulcanization: put the product into a high temperature box for secondary vulcanization, step by step increase the temperature to 200°C, and maintain for 12 hours.