Near-equimolar-ratio multi-principal-element metal oxide anticorrosive coating as well as preparation method and application of approximately-equimolar-ratio multi-principal-element metal oxide anticorrosive coating

By using nearly equimolar ratio of multi-main metal oxide anticorrosion coating (AlTiZrNiCr)Ox in concentrated solar thermal power generation systems, the high temperature molten salt corrosion problem is solved, significantly reducing the corrosion rate and extending the life of system components.

CN118879103AActive Publication Date: 2024-11-01UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202410945228.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-01
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The corrosion rate of molten salt in high-temperature operating environments is accelerated, and the existing technology is difficult to effectively control the corrosion rate, which affects the reliability and life of the system.

Method used

A multi-maintenance metal oxide anticorrosion coating (AlTiZrNiCr)Ox with a nearly equal molar ratio is deposited on the surface of stainless steel through target material preparation and magnetron sputtering technology to form an anticorrosion coating with controllable thickness to slow down molten salt corrosion.

Benefits of technology

It effectively reduces the corrosion rate by more than 50%, extends the service life of system components, and provides a new material system for molten salt corrosion control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879103A_ABST
    Figure CN118879103A_ABST
Patent Text Reader

Abstract

The invention provides an approximately equimolar-ratio multi-principal-element metal oxide anticorrosive coating as well as a preparation method and application thereof, and belongs to the technical field of fused salt corrosion related to concentrating solar thermal power generation. The chemical composition of the coating is (AlTiZrNiCr) Ox, and the coating comprises the following elements in percentage by atom: 5-15 at% of Al, 5-15 at% of Ti, 8-12 at% of Zr, 5-15 at% of Ni, 5-15 at% of Cr and the balance of O and a very small amount of C and nitrogen, and x is equal to 1-2. The coating is applied to the surface of an alloy sample based on stainless steel, and is tested in a related fused salt environment of a concentrating solar thermal power generation system, so that the high-temperature fused salt corrosion of a structural material can be effectively controlled. Based on the test result of the embodiment, the coating can effectively reduce the corrosion rate by more than 50%, and can effectively prolong the service life of a CSP system and other related material components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of molten salt corrosion involved in concentrated solar thermal power generation, and particularly relates to a multi-principal metal oxide anti-corrosion coating with a nearly equal molar ratio, a preparation method thereof and an application thereof in a molten salt environment. Background Art

[0002] Over the past decade, concentrated solar thermal power (CSP) technology has developed rapidly. From 2010 to 2015, its installed capacity grew by about 50% annually, reaching a total global installed capacity of about 5 GW, which can provide electricity for nearly 4 million households. 2 -KCl-NaCl·nH 2 O) With the development of heat storage media, CSP systems can operate at temperatures up to 800°C, significantly increasing power generation capacity. However, this high-temperature operating environment leads to accelerated molten salt corrosion in the thermal storage tanks, circulation loops, and heat exchangers of CSP systems. These components are typically constructed using 310 stainless steel, Inconel 800, and Hastelloy (Ha) C-276. Even the most corrosion-resistant Hastelloy Ha C-276 has a corrosion rate of more than 0.5 mm / year. Therefore, there is an urgent need to find a way to control the corrosion rate to improve the reliability of the system, making it a more competitive energy source with fossil fuel energy and potentially alleviating the challenges of energy storage.

[0003] Multi-principal cermets such as high entropy carbides are relatively new materials that possess a variety of excellent properties, including good wear resistance, high hardness, and excellent oxidation / corrosion resistance. For example, (AlTiVCr)O x It has been shown to reduce the corrosion rate of metal substrates in saline solutions to 1 µm per year. However, research on the use of multi-principal metal oxides as corrosion-resistant coatings is still limited; to date, there are no research reports or patents on multi-principal metal oxides in high-temperature application environments. Summary of the invention

[0004] In order to solve the high temperature application technical problems existing in the prior art, the present invention provides a new type of multi-principal metal oxide coating with nearly equal molar ratio, with (AlTiZrNiCr)O x The thin film coating is expected to combine the superior properties of a single oxide component, namely passivation, diffusion resistance, hardness, adhesion and shape memory effect, to alleviate the corrosion of metals in molten salt environments.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] The present invention provides a multi-principal metal oxide anti-corrosion coating with a nearly equal molar ratio, the chemical composition of which is (AlTiZrNiCr)O x The atomic percentage of each element is as follows: 5-15 at% Al, 5-15 at% Ti, 8-12 at% Zr, 5-15 at% Ni, 5-15 at% Cr, the rest is O and very small amounts of C and N, and x=1-2.

[0007] Furthermore, in the coating, the atomic percentage of O is 40-55 at%, and the atomic percentage of C and nitrogen is 2-5 at%.

[0008] For comparison, two additional sputtering targets are prepared in the specific embodiment of the present invention, which are TiZrNiCr and pure Al materials, respectively, to deposit multi-principal oxide coatings with non-equimolar ratios as a comparative example.

[0009] Preferably, the atomic percentage of each element in the oxide anti-corrosion coating is as follows: 7-8 at% Al, 6-7 at% Ti, 9-10 at% Zr, 6-9 at% Ni, 6-9 at% Cr, 40-55 at% O, and x = 1. The atomic percentage of carbon and nitrogen in the coating is 2-5 at%.

[0010] The present invention also provides a method for preparing the multi-principal metal-based oxide anti-corrosion coating, comprising the following steps:

[0011] (1) Target material preparation: Al, Ti, Cr, Zr, and Ni powders in equal molar ratios are mixed, ball-milled, placed in a graphite mold, and sintered using spark plasma sintering technology to obtain AlTiCrZrNi target material;

[0012] For comparison, the same method was used in the comparative example to prepare two additional sputtering targets, namely TiZrNiCr (25at%) and pure Al, for depositing non-equimolar multi-principal oxide-aluminum-rich multi-principal coatings.

[0013] Preferably, the amount of Al, Ti, Cr, Zr and Ni powders is 20 at %.

[0014] Preferably, the ball milling is carried out in a high-energy ball mill, the ball milling time is 15-25 hours, and the ball milling speed is 100-300 rpm. Preferably, the ball milling time is 20 hours, and the ball milling speed is 200 rpm.

[0015] Preferably, the sintering temperature is 800-1000°C and the pressure is 40-60 MPa. Preferably, the sintering temperature is 900°C and the pressure is 50 MPa.

[0016] Preferably, the target material has dimensions of 3 inches in diameter and 0.25 inches in thickness.

[0017] (2) Pre-sputtering:

[0018] The AlTiCrZrNi target prepared in step (1) is loaded into a magnetron sputtering device, and the vacuum degree of the chamber is evacuated to 5 mTorr at room temperature to start pre-sputtering to remove impurities on the surface of the target and peel off the oxide film;

[0019] Preferably, the matrix material is selected from at least one of stainless steel, nickel alloy, titanium alloy and zinc alloy.

[0020] Preferably, the pre-sputtering process parameters are: Ar as the working gas, the gas flow rate is 20 ccm, the sputtering power is 150 W, and the sputtering time is 2-3 min.

[0021] (3) Coating deposition: Place the substrate material into the magnetron sputtering equipment, open the sputtering baffle, and adjust the gas flow rate to 19.7 sccm Ar and 4.80 sccm O. 2 , the power was adjusted to 150W to start sputtering, and the pressure in the deposition chamber was 5mTorr.

[0022] Preferably, the coating thickness is 1-5 microns, preferably 2 microns.

[0023] The present invention also provides application of the multi-principal metal oxide anti-corrosion coating with nearly equal molar ratio in a molten salt environment.

[0024] The beneficial effects brought about by the technical solution provided by the present invention include at least:

[0025] The present invention provides a novel multi-principal metal oxide (AlTiZrNiCr)O x The coating is applied to the surface of a stainless steel-based alloy sample and tested in a molten salt environment of a related concentrated solar thermal power generation system, which can effectively control the high-temperature molten salt corrosion of structural materials. Based on the test results of the embodiment, the coating can effectively reduce the corrosion rate by more than 50%, and can effectively extend the service life of the CSP system and other related material components.

[0026] The multi-principal metal oxide coating is used for the first time to test molten salt corrosion, providing a new material system for molten salt corrosion control. It has novel composition and simple preparation process. Through magnetron sputtering deposition, a coating with controllable composition, structure and thickness and no heterogeneous structure can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0028] FIG1 is a morphology and composition analysis of the coating surface of Example 1, wherein FIG1(a) is a SEM image of the coating morphology, and FIG1(b) is a SEM / EDS analysis image of the coating;

[0029] Figure 2 is a comparison of the states of the 310L sample with coating and the control sample in Example 1, as well as the high-aluminum coating sample in Comparative Example 1 before and after corrosion in molten salt, wherein Figure 2 (a) is the corrosion potential test result, and Figure 2 (b) is the Fe 2+ Concentration (wt.%) test results. DETAILED DESCRIPTION

[0030] In order to make the invention purpose, technical scheme and beneficial technical effect of the present invention clearer, the present invention is described in detail below in conjunction with specific embodiments. It should be understood that the embodiments described in this specification are only for explaining the present invention, not for limiting the present invention.

[0031] Example 1

[0032] (1) Substrate material selection: Considering that stainless steel 310L is more susceptible to corrosion than nickel alloy, it is most convincing to use it as the substrate material of the coating to test the corrosion resistance of the coating. According to the ASTM A967 standard, the stainless steel substrate is pre-treated with acid to remove the surface oxide film.

[0033] (2) Target preparation: Al, Ti, Cr, Zr, and Ni powders in equal molar ratios (20 at%) were mixed and milled in a high-energy ball mill for 20 hours at a speed of 200 rpm. The milled nanopowders were placed in a graphite mold and sintered using spark plasma sintering technology. The sintering temperature was 900°C and the pressure was 50 MPa. The target size was 3 inches in diameter and 0.25 inches in thickness.

[0034] (3) Pre-sputtering: The target prepared in step (2) is loaded into a magnetron sputtering device, and the vacuum of the chamber is evacuated to 5 mTorr at room temperature to start pre-sputtering. Ar is used as the working gas, the gas flow rate is 20 ccm, the sputtering power is 150 W, and the sputtering time is 2-3 min. The purpose is to peel off the oxide film.

[0035] (4) Coating deposition: The target material and substrate material obtained above were deposited in an Ar-25%O 2Reactive magnetron sputtering technology was used in the environment to deposit a coating with a target thickness of about 2 microns on the surface of the substrate material. The gas flow rate was controlled at 19.7 sccm Ar and 4.80 sccm O 2 The deposition chamber pressure was about 5 mTorr and the sputtering power was 150W.

[0036] Comparative Example 1

[0037] In step (2): two sputtering targets were prepared by the same target material preparation method, namely TiZrNiCr (25 at %) and pure Al. The other processes were the same as in Example 1, and a non-equimolar multi-principal oxide-aluminum-rich multi-principal coating was prepared.

[0038] The size of the 310L sample deposited with a coating of nearly equal molar ratio in Example 1, the sample deposited with a non-equal molar ratio of aluminum-rich coating in Comparative Example 1, and the control sample sample without deposited coating are all 5 mm×80 mm×2 mm. The SEM morphology of the surface of the coating of nearly equal molar ratio in Example 1 is shown in Figure 1(a), and it can be seen that the surface is flat and has no pores. The EDS (X-ray energy spectrum) component distribution of the coating surface is shown in Figure 1(b), indicating that the distribution of each element in the coating is uniform.

[0039] The EDS analysis results of the nearly equimolar ratio coating of Example 1 are shown in Table 1. It can be seen that the microstructure and composition of the deposited oxide film are uniformly distributed, without segregation and the appearance of the second phase, and the five metal elements are basically distributed in equimolar amounts, following the basic definition and expectation of multi-principal metal oxides (here specifically high entropy oxides). The total atomic percentage of the elements is less than 100% because a part of them is a stainless steel substrate component (mainly Fe), which is not listed in the table.

[0040] Table 1 EDS analysis results of the coating with nearly equal molar ratio in Example 1

[0041]

[0042] The XPS (X-ray photoelectron spectroscopy) analysis results of the nearly equimolar ratio coating of Example 1 are shown in Table 2, indicating that the metal elements mainly exist in the oxidized form, such as Al 2 O 3 、ZrO 2 、TiO 2 / TiO, NiO, Cr 2 O 3 In addition, after XPS sputtering for 20 minutes, the film coating still contains about 1-5 at% carbon, indicating that the element itself is likely to be a trace component of the film, that is, the coating can be expressed as (AlTiZrNiCr)O xin the form of, where x = 1-2, and the carbon and nitrogen contents in the film are 2-5at%.

[0043] Table 2 XPS analysis results (at.%)

[0044]

[0045] The EDS analysis results of the non-equimolar ratio aluminum-rich coating of Comparative Example 1 are shown in Table 3. It can be seen that the aluminum content in the deposited oxide film is much higher than that of other metal elements, and the five metal elements are distributed in non-equimolar amounts.

[0046] Table 3 EDS analysis results of non-equimolar ratio coatings in Comparative Example 1

[0047]

[0048] The anti-corrosion properties of the coatings obtained in Example 1, Comparative Example 1, and the control sample without the deposited coating were evaluated: 57 wt% MgCl 2 -21 wt% KCl-22 wt% NaCl·nH 2 The corrosion resistance of the molten salt environment reactor was evaluated by connecting an external electrochemical workstation. The reference electrode was Ag / AgCl / MgO. The entire molten salt corrosion device was placed in a glove box and protected by inert argon gas. After the molten salt was kept at a constant temperature for 24 hours, the 310L sample with coating and the reference 310L sample coupon were placed in the molten salt tank for corrosion potential monitoring. The monitoring time was 7 days.

[0049] During this period, the potential evolution process with time is shown in Figure 2 (a), indicating that the potential changes of the coated and uncoated samples tend to be stable, and the coated sample of Example 1 presents a higher potential, and the open circuit potential of the coated sample of Comparative Example 1 is the lowest, which accelerates the corrosion rate to a certain extent. The applicant believes that the reason is that the electrochemical activity of aluminum is more active than that of several other elements, that is, the electrochemical corrosion potential is lower. Therefore, in the test molten salt environment, the aluminum-rich coating is more inclined to dissolve than the nearly equimolar ratio coating, resulting in a decrease in the overall corrosion resistance of the coating. Therefore, not all oxide coatings containing the same or similar elements in this application have good corrosion resistance.

[0050] After the corrosion experiment, some molten salt samples were taken for ICP-OES analysis. The results are shown in Figure 2(b), which shows that the Fe 2+ The content is relatively low, indicating that the equimolar ratio multi-principal coating can provide an anti-corrosion barrier for the base material 310L and effectively reduce the corrosion rate of 310L. 2+ The content is the highest, which is consistent with the potential evolution trend in Figure 2(a).2+ Based on Faraday's law, combined with some physical parameters, such as the iron content of stainless steel is about 60wt%, the density is 8g / cm 3 、The corrosion area of ​​the sample is 10cm 2 , corrosion time is 7 days, it can be estimated that the absolute corrosion rates of the coated and uncoated samples are approximately 0.45 mm / year and 1 mm / year, respectively, that is, the coating can significantly reduce the corrosion rate of the substrate.

[0051] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art who is familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A multi-principal metal oxide anti-corrosion coating with nearly equal molar ratio, characterized in that: The chemical composition of the coating is (AlTiZrNiCr)O x The atomic percentage of each element is as follows: 5-15 at% Al, 5-15 at% Ti, 8-12 at% Zr, 5-15 at% Ni, 5-15 at% Cr, and the rest is O, very small amounts of C and N, and x=1-2.

2. The coating according to claim 1, characterized in that In the coating, the atomic percentage of O is 40-55 at%, and the atomic percentage of C and N is 2-5 at%.

3. The coating according to claim 1 or 2, characterized in that The atomic percentage of each element in the oxide anti-corrosion coating is as follows: 7-8 at% Al, 6-7 at% Ti, 9-10 at% Zr, 6-9 at% Ni, 6-9 at% Cr, 40-55 at% O, and x=1; the atomic percentage of carbon and nitrogen in the coating is 2-5 at%.

4. The method for preparing the multi-principal metal-based oxide anti-corrosion coating according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Target material preparation: Al, Ti, Cr, Zr, and Ni powders in equal molar ratios are mixed, ball-milled, placed in a graphite mold, and sintered using spark plasma sintering technology to obtain AlTiCrZrNi target material; (2) Pre-sputtering: The AlTiCrZrNi target prepared in step (1) is loaded into a magnetron sputtering device, and the vacuum degree of the chamber is evacuated to 5 mTorr at room temperature to start pre-sputtering to remove impurities on the surface of the target and peel off the oxide film; (3) Coating deposition: Load the substrate material into the magnetron sputtering equipment, open the sputtering baffle, adjust the gas flow rate to 19.7 sccm Ar, 4.80 sccm O2, adjust the power to 150 W to start sputtering, and the deposition chamber pressure is 5 mTorr.

5. The preparation method according to claim 4, characterized in that: In step (1), the amount of Al, Ti, Cr, Zr and Ni powders used is 20 at %.

6. The preparation method according to claim 4, characterized in that: In step (1), the ball milling is carried out in a high-energy ball mill, the ball milling time is 15-25 hours, and the ball milling speed is 100-300 rpm; the sintering temperature is 800-1000°C, and the pressure is 40-60 MPa.

7. The preparation method according to claim 4, characterized in that: In step (2), the base material is selected from at least one of stainless steel, nickel alloy, titanium alloy and zinc alloy.

8. The preparation method according to claim 4, characterized in that: In step (2), the pre-sputtering process parameters are: Ar as the working gas, the gas flow rate is 20 ccm, the sputtering power is 150 W, and the sputtering time is 2-3 min.

9. The preparation method according to claim 4, characterized in that: In step (3), the coating thickness is 1-5 microns.

10. Use of the multi-principal metal oxide anti-corrosion coating with nearly equal molar ratios as described in any one of claims 1 to 3 in a molten salt environment.

Citation Information

Patent Citations

  • High-property optothermal transformation multiple-element alloy nitride film and preparation method thereof

    CN104630706A

  • Cooking utensil and preparation method thereof

    CN114645238A

  • Anti-corrosion and anti-hydrogen permeation coating and preparation method thereof

    CN114686810A

  • High-entropy alloy powder and preparation method thereof and high-entropy alloy laser cladding layer and preparation method thereof

    CN114875291A

  • Zirconium alloy based AlCrNbTiZr high-entropy alloy coating resistant to high-temperature water corrosion and preparation method thereof

    CN115305444A

Cited By

  • A method for preparing a high-temperature molten salt corrosion-resistant boronized layer on a stainless steel surface and a stainless steel product

    CN122979815A