Fluorenyl-containing anti-dazzle coating, preparation method thereof, anti-dazzle film and polarizer

CN118879189AActive Publication Date: 2024-11-01ANHUI HEMEI MATERIALS TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411173418.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-01
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

[0004]为了解决现有技术中粒子分布不均匀、闪点较重、耐磨擦和硬度较差的问题,本发明提供了一种含芴基防眩涂料及其制备方法、防眩膜、偏光片

Benefits of technology

[0025] In order to achieve the above object, the present application also provides an anti-glare film, which includes a film layer prepared from the above-mentioned fluorene-based anti-glare coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010742060000121
    Figure BDA0005010742060000121
  • Figure BDA0005010742060000131
    Figure BDA0005010742060000131
Patent Text Reader

Abstract

The invention provides a fluorenyl-containing anti-dazzle coating and a preparation method thereof, an anti-dazzle film and a polaroid, in the preparation process of the fluorenyl-containing anti-dazzle coating, micron-scale and nano-scale silicon dioxide with different particle sizes are selected as dispersion particles, after fluorenyl grafting modification treatment is carried out on the dispersion particles, reaction is introduced in batches in the pre-polymerization and chain extension process, and the fluorenyl-containing anti-dazzle coating is obtained. According to the anti-glare coating, the dispersity of particles on a coating substrate is enhanced, protrusions and flash points caused by agglomeration among the particles are avoided, the anti-glare visual effect is achieved, meanwhile, the micron-scale particles and the nano-scale particles can be distributed in a staggered and ordered mode, on one hand, the dispersion uniformity is further improved, light diffuse reflection is enhanced and uniform, and on the other hand, the anti-glare effect is improved. Grafted particles serve as reaction monomers to enter cross-linking polymerization of a polymer, so that the wear resistance and hardness of a coating are enhanced to a great extent, and the problem that the surface of a traditional anti-dazzle film is prone to brittleness and cracking is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical films, in particular to a fluorene-based anti-glare coating and a preparation method thereof, as well as an anti-glare film and a polarizer comprising the fluorene-based anti-glare coating layer. Background Art

[0002] The display module is mainly composed of polarizer and liquid crystal structure, among which polarizer is an indispensable key component in LCD and OLED display. However, when strong outdoor sunlight or indoor lighting is projected onto the display screen, it is easy to produce specular reflection glare. Therefore, in order to reduce the reflection of surrounding light sources and improve the brightness and clarity of the image, it is necessary to make certain treatments on the surface of the display to diffuse the light emitted from the light source inside the display, and at the same time reduce the positive reflection effect of the light incident from the outside of the display, so as to alleviate the visual fatigue caused by long-term use.

[0003] Therefore, anti-glare films are widely used in display devices. The concave-convex microstructure on the surface realizes diffuse reflection of incident strong light, thereby achieving the effect of anti-glare and improving display effect. Generally, the anti-glare coating is coated on the surface of the base film of the polarizer protective film, and the anti-glare film can be obtained after light curing or heat curing. However, the anti-glare film often has problems such as surface protrusions, heavy flash point, poor clarity, etc. due to the influence of the particle size matching of the diffusion particles and the uniformity of particle distribution, which will greatly affect the display effect of the display screen. For example, in the patent application document of publication number CN115505327B, an anti-glare layer is formed by using organic-inorganic composite microspheres and an acrylic resin with a suitable shrinkage rate, but its particle distribution is uneven, the friction resistance is poor, the hardness is low, and there is a problem of brittle fracture of the film surface. Summary of the invention

[0004] In order to solve the problems of uneven particle distribution, heavy flash point, poor abrasion resistance and hardness in the prior art, the present invention provides a fluorene-based anti-glare coating and a preparation method thereof, an anti-glare film and a polarizer.

[0005] To achieve the above objectives, this application is implemented through the following technical solutions:

[0006] The present application provides a method for preparing a fluorene-based anti-glare coating, comprising the following steps:

[0007] S1. Under a nitrogen atmosphere, 25 to 30 parts of polyisocyanate, 0.5 to 0.6 parts of fluorenyl-modified silica-a, and 150 to 200 parts of polytetrahydrofuran diol are added to a reaction container by weight, and a prepolymerization reaction is carried out at 82 to 88° C. for 2 to 2.5 hours, and then the temperature is cooled to room temperature, and 5 to 8 parts of hydroxyethyl acrylate are added, and the temperature is raised to 72 to 74° C. and the reaction is continued for 3 to 5 hours;

[0008] S2, adding 2 to 6 parts of chain extender, 5 to 10 parts of methyl methacrylate, 0.2 to 0.6 parts of fluorenyl-modified silica-b, and 0.02 to 0.07 parts of azobisisobutyronitrile to the solution after the reaction in step S1, by weight, and performing a chain extension reaction at 68 to 73° C. for 2.5 to 3 hours;

[0009] S3, cooling to room temperature, adding triethylamine to neutralize for 25 to 35 minutes, then adding deionized water, and high-speed shearing at 800 to 1000 rpm for 22 to 26 minutes to obtain a fluorene-containing anti-glare coating;

[0010] Wherein: the fluorenyl-modified silica-a in step S1 is prepared from silica with a particle size of 1 to 5 μm, and the fluorenyl-modified silica-b in step S2 is prepared from silica with a particle size of 400 to 600 nm.

[0011] Based on the above technical scheme, the present application selects silicon dioxide with two different particle sizes, micron and nanometer, as dispersed particles, and performs fluorene grafting modification treatment on them, and introduces reactions in the prepolymerization and chain extension processes respectively. This not only enhances the dispersibility of the particles in the coating substrate, avoids the agglomeration between particles to produce protrusions and flash points, and achieves an anti-glare visual effect. At the same time, the micron-sized particles and nanometer-sized particles can be staggered and distributed in an orderly manner. On the one hand, its dispersion uniformity is further improved, and the diffuse reflection of light is enhanced and uniform. On the other hand, the grafted particles enter the cross-linking polymerization of the polymer as reaction monomers, which greatly enhances the wear resistance and hardness of the coating, and overcomes the problem of brittle cracking of the surface of traditional anti-glare films.

[0012] As a further improvement of the present application, the fluorene-modified silica-a is prepared by the following method:

[0013] By weight, 3 to 5 parts of γ-aminopropyltriethoxysilane and 5 to 6 parts of silicon dioxide with a particle size of 1 to 5 μm are added to 80 to 100 parts of deionized water, reacted at 78 to 82° C. and 100 to 120 rpm for 1 to 2 hours, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane;

[0014] By weight, 3 to 5 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene are dissolved in 80 to 100 parts of toluene solution, and 5 to 10 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica are added. Under nitrogen protection, 100 to 110 ml of a toluene solution containing 0.5 to 0.7% azobisisobutyronitrile is added at a rate of 20 ml / h. The mixture is reacted at 78 to 82° C. and 20 to 50 rpm for 13 to 15 hours. The mixture is cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorene-modified silica-a.

[0015] Based on the above further improved technical solution, γ-aminopropyltriethoxysilane is used to treat silica, and its alkoxy group is hydrolyzed to form a silanol group (Si-OH), which is then dehydrated and condensed with the hydroxyl group on the surface of silica to form a covalently bonded silicon oxygen bond (Si-O-Si), which is grafted onto the surface of silica; then 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene is added, and the molecule contains a hydroxyethoxy group (i.e. -OCH2CH2OH), in which the hydroxyl group (-OH) is a potential active group, which can react with γ-aminopropyltriethoxysilane and the silicon hydroxyl group (Si-OH) on the surface of silica, and be grafted onto the surface of silica. Due to the presence of the fluorene group, the grafted silica particles have a certain scattering effect on light, which can reduce the light intensity, thereby reducing the glare phenomenon, and at the same time, help to improve the wear resistance of the coating.

[0016] As a further improvement of the present application, the preparation of the fluorenyl-modified silica-a also includes a silica pretreatment step, which is as follows: adding silica with a particle size of 1 to 5 μm to a sodium hydroxide solution with a pH of 10 to 12, adding anhydrous ethanol thereto, alkaline etching at 70 to 80° C. and 35 to 45 rpm for 1 to 2 hours, filtering, rinsing, and drying at 100 to 104° C. for 10 to 12 hours to obtain pretreated silica.

[0017] Based on the above further improved technical solution, alkaline etching of silicon dioxide can increase its surface roughness and introduce some surface defects, such as vacancies, dangling bonds, etc. These defects usually have high reactivity because they are in an energy unstable state and easily react with other substances, which is beneficial to improve the subsequent grafting reaction rate. Adding ethanol during the process helps to reduce the difference in etching rate caused by different density and improve the etching effect.

[0018] As a further improvement of the present application, the fluorene-modified silica-b is prepared by the following method:

[0019] By weight, 3 to 5 parts of γ-aminopropyltriethoxysilane and 5 to 6 parts of silicon dioxide with a particle size of 400 to 600 nm are added to 80 to 100 parts of deionized water, reacted at 78 to 82° C. and 100 to 120 rpm for 1 to 2 hours, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane;

[0020] By weight, 3 to 5 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene are dissolved in 80 to 100 parts of toluene solution, and 5 to 10 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica are added. Under nitrogen protection, 100 to 110 ml of toluene solution containing 0.5 to 0.7% azobisisobutyronitrile is added at a rate of 20 ml / h. The reaction is carried out at 78 to 82°C and 20 to 50 rpm for 13 to 15 hours, and then cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorenyl-modified silica-b. The reaction principle and function of fluorenyl modification of silica-b refer to the fluorenyl modification of silica-a.

[0021] As a further improvement of the present application, the preparation of the fluorene-modified silica-b also includes a step of silica pretreatment, which is as follows: adding silica with a particle size of 400 to 600 nm to a sodium hydroxide solution with a pH of 10 to 12, adding anhydrous ethanol thereto, alkaline etching at 70 to 80°C and 35 to 45 rpm for 1 to 2 hours, filtering, rinsing, and drying at 100 to 104°C for 10 to 12 hours to obtain pretreated silica. The principle and effect of alkaline etching of silica-b refer to the alkaline etching of silica-a.

[0022] As a further improvement of the present application, in step S1, the polyisocyanate is selected from one or more of toluene diisocyanate, diphenylmethane diisocyanate, and isophorone diisocyanate.

[0023] As a further improvement of the present application, in step S2, the chain extender is selected from one or more of 1,4-butanediol, ethylene glycol, propylene glycol, and 1,4-cyclohexanediol.

[0024] To achieve the above objectives, the present application also provides a fluorene-based anti-glare coating, which is prepared by the method described above.

[0025] To achieve the above objectives, the present application also provides an anti-glare film, which comprises a film layer prepared from the above-mentioned fluorene-containing anti-glare coating.

[0026] To achieve the above objectives, the present application also provides a polarizer, which includes the anti-glare film mentioned above.

[0027] The beneficial effect of the present application is that the present application provides an anti-glare coating containing fluorene groups and a preparation method thereof, wherein: polyisocyanate and polytetrahydrofuran diol are subjected to a prepolymerization reaction to generate a polyurethane prepolymer, and then hydroxyethyl acrylate is added to participate in the prepolymerization to generate a polyurethane acrylic prepolymer. During the polyurethane acrylic prepolymerization process, large-particle fluorene-modified silica-a is added to participate in the reaction with polyisocyanate and polyol to enter the prepolymer, and then hydroxyethyl acrylate is added, and the hydroxyl group therein reacts with the unreacted isocyanate group in the prepolymer, and at the same time, the C=C double bond and fluorene group in the hydroxyethyl acrylate are introduced into the polyurethane molecular chain; during the chain extension process, small-particle fluorene-modified silica-b is added, and under the action of a catalyst, it can be used as a chain extender to extend the molecular chain of the polyurethane acrylic prepolymer, enhance its polymerization crosslinking, achieve staggered and orderly distribution of silica particles of different particle sizes, improve the density and hardness of the coating, eliminate the flash point, and enhance the adhesion between the coating and the substrate. The anti-glare film and polarizer prepared from the fluorene-containing anti-glare coating have excellent hardness, adhesion, wear resistance and display effect. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the implementation of the present invention clearer, the specific implementation methods of the present invention are clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] Preparation of fluorene-modified silica-a:

[0031] By weight, 3 parts of γ-aminopropyltriethoxysilane and 5 parts of silicon dioxide with a particle size of 1 μm were added to 80 parts of deionized water, reacted at 78° C. and 100 rpm for 1 hour, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane;

[0032] By weight, 3 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene are dissolved in 80 parts of toluene solution, and 5 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica are added. Under nitrogen protection, 100 ml of a toluene solution containing 0.5% azobisisobutyronitrile is added at a rate of 20 ml / h. The mixture is reacted at 78°C and 20 rpm for 13 hours, cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorene-modified silica-a.

[0033] Preparation of fluorene-modified silica-b:

[0034] By weight, 3 parts of γ-aminopropyltriethoxysilane and 5 parts of silicon dioxide with a particle size of 400 nm were added to 80 parts of deionized water, reacted at 78° C. and 100 rpm for 1 hour, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane;

[0035] By weight, 3 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene were dissolved in 80 parts of toluene solution, and 5 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica were added. Under nitrogen protection, 100 ml of a toluene solution containing 0.5% azobisisobutyronitrile was added at a rate of 20 ml / h. The mixture was reacted at 78°C and 20 rpm for 13 hours, cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorene-modified silica-b.

[0036] The preparation method of the fluorene-containing anti-glare coating comprises the following steps:

[0037] S1. Under a nitrogen atmosphere, 25 parts of toluene diisocyanate, 0.5 parts of fluorenyl-modified silica-a, and 150 parts of polytetrahydrofuran diol were added into a reaction container by weight, and prepolymerized at 82° C. for 2 hours, then cooled to room temperature, and 5 parts of hydroxyethyl acrylate were added, and the temperature was raised to 72° C. and reacted for another 3 hours;

[0038] S2, adding 2 parts of 1,4-butanediol, 5 parts of methyl methacrylate, 0.2 parts of fluorenyl-modified silica-b, and 0.02 parts of azobisisobutyronitrile to the solution after the reaction in step S1, and performing a chain extension reaction at 68° C. for 2.5 hours;

[0039] S3, cool to room temperature, add triethylamine to neutralize for 25 minutes, then add deionized water, and high-speed shear at 800 rpm for 22 minutes to obtain a fluorene-containing anti-glare coating.

[0040] Example 2

[0041] Preparation of fluorene-modified silica-a:

[0042] By weight, 4 parts of γ-aminopropyltriethoxysilane and 5 parts of silicon dioxide with a particle size of 3 μm were added to 90 parts of deionized water, reacted at 79° C. and 105 rpm for 1.2 hours, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane;

[0043] By weight, 4 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene were dissolved in 90 parts of toluene solution, and 6 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica were added. Under nitrogen protection, 105 ml of a toluene solution containing 0.6% azobisisobutyronitrile was added at a rate of 20 ml / h. The mixture was reacted at 79° C. and 25 rpm for 14 hours, cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorene-modified silica-a.

[0044] Preparation of fluorene-modified silica-b:

[0045] By weight, 4 parts of γ-aminopropyltriethoxysilane and 5 parts of silicon dioxide with a particle size of 500 nm were added to 90 parts of deionized water, reacted at 79° C. and 105 rpm for 1.2 hours, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane;

[0046] By weight, 4 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene were dissolved in 90 parts of toluene solution, and 6 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica were added. Under nitrogen protection, 105 ml of a toluene solution containing 0.6% azobisisobutyronitrile was added at a rate of 20 ml / h. The mixture was reacted at 79° C. and 25 rpm for 14 hours, cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorene-modified silica-b.

[0047] The preparation method of the fluorene-containing anti-glare coating comprises the following steps:

[0048] S1. Under a nitrogen atmosphere, 28 parts of toluene diisocyanate, 0.6 parts of fluorenyl-modified silica-a, and 160 parts of polytetrahydrofuran diol were added into a reaction container by weight, and prepolymerized at 83° C. for 2.2 hours, then cooled to room temperature, and 6 parts of hydroxyethyl acrylate were added, and the temperature was raised to 73° C. and reacted for another 3.5 hours;

[0049] S2, adding 2.5 parts of 1,4-butanediol, 6 parts of methyl methacrylate, 0.3 parts of fluorenyl-modified silica-b, and 0.03 parts of azobisisobutyronitrile to the solution after the reaction in step S1, and performing a chain extension reaction at 69° C. for 2.8 hours;

[0050] S3, cool to room temperature, add triethylamine to neutralize for 25 minutes, then add deionized water, and high-speed shear at 800 rpm for 22 minutes to obtain a fluorene-containing anti-glare coating.

[0051] Example 3

[0052] Preparation of fluorene-modified silica-a:

[0053] By weight, 5 parts of γ-aminopropyltriethoxysilane and 6 parts of silicon dioxide with a particle size of 5 μm were added to 100 parts of deionized water, reacted at 82° C. and 120 rpm for 2 hours, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane;

[0054] By weight, 5 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene are dissolved in 100 parts of toluene solution, and 10 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica are added. Under nitrogen protection, 110 ml of a toluene solution containing 0.7% azobisisobutyronitrile is added at a rate of 20 ml / h. The mixture is reacted at 82°C and 50 rpm for 15 hours, cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorene-modified silica-a.

[0055] Preparation of fluorene-modified silica-b:

[0056] By weight, 5 parts of γ-aminopropyltriethoxysilane and 6 parts of silicon dioxide with a particle size of 600 nm were added to 100 parts of deionized water, reacted at 82° C. and 120 rpm for 2 hours, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane;

[0057] By weight, 5 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene were dissolved in 100 parts of toluene solution, and 10 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica were added. Under nitrogen protection, 110 ml of a toluene solution containing 0.7% azobisisobutyronitrile was added at a rate of 20 ml / h. The mixture was reacted at 82°C and 50 rpm for 15 hours, cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorene-modified silica-b.

[0058] The preparation method of the fluorene-containing anti-glare coating comprises the following steps:

[0059] S1. Under a nitrogen atmosphere, 30 parts of toluene diisocyanate, 0.6 parts of fluorenyl-modified silica-a, and 200 parts of polytetrahydrofuran diol were added into a reaction container by weight, and prepolymerized at 88° C. for 2.5 hours, then cooled to room temperature, and then 8 parts of hydroxyethyl acrylate were added, and the temperature was raised to 74° C. for further reaction for 5 hours;

[0060] S2, adding 6 parts of 1,4-butanediol, 10 parts of methyl methacrylate, 0.6 parts of fluorenyl-modified silica-b, and 0.07 parts of azobisisobutyronitrile to the solution after the reaction in step S1, and performing a chain extension reaction at 73° C. for 3 hours;

[0061] S3, cool to room temperature, add triethylamine to neutralize for 35 minutes, then add deionized water, and high-speed shear at 1000 rpm for 26 minutes to obtain a fluorene-containing anti-glare coating.

[0062] Example 4

[0063] The difference between this embodiment and embodiment 3 is that:

[0064] 1) The preparation of fluorene-modified silica-a also includes a pretreatment step of silica: adding silica with a particle size of 5 μm to a sodium hydroxide solution with a pH of 12, adding anhydrous ethanol thereto, alkaline etching at 80° C. and 45 rpm for 2 h, filtering, rinsing, and drying at 104° C. for 12 h to obtain pretreated silica;

[0065] 2) The preparation of fluorene-modified silica-b also includes a pretreatment step of silica: silica with a particle size of 600 nm is added to a sodium hydroxide solution with a pH of 12, anhydrous ethanol is added thereto, alkaline etching is performed at 80°C and 45 rpm for 2 hours, filtering, rinsing, and drying at 104°C for 12 hours to obtain pretreated silica.

[0066] Example 5

[0067] The difference between this embodiment and embodiment 3 is that:

[0068] 1) The preparation of fluorene-modified silica-a also includes a pretreatment step of silica: adding silica with a particle size of 5 μm to a sodium hydroxide solution with a pH of 10, adding anhydrous ethanol thereto, alkaline etching at 70° C. and 35 rpm for 1 hour, filtering, rinsing, and drying at 100° C. for 10 hours to obtain pretreated silica;

[0069] 2) The preparation of fluorenyl-modified silica-b also includes a pretreatment step of silica: silica with a particle size of 600 nm is added to a sodium hydroxide solution with a pH of 10, anhydrous ethanol is added thereto, alkaline etching is performed at 70°C and 35 rpm for 1 hour, filtering, rinsing, and drying at 100°C for 10 hours to obtain pretreated silica.

[0070] Example 6

[0071] The difference between this embodiment and embodiment 3 is that:

[0072] 1) The preparation of fluorene-modified silica-a also includes a pretreatment step of silica: adding silica with a particle size of 5 μm to a sodium hydroxide solution with a pH of 11, adding anhydrous ethanol thereto, alkaline etching at 72° C. and 36 rpm for 1.5 h, filtering, rinsing, and drying at 102° C. for 11 h to obtain pretreated silica;

[0073] 2) The preparation of fluorene-modified silica-b also includes a pretreatment step of silica: silica with a particle size of 600 nm is added to a sodium hydroxide solution with a pH of 11, anhydrous ethanol is added thereto, alkaline etching is performed at 72°C and 36 rpm for 1.5 h, filtering, rinsing, and drying at 102°C for 11 h to obtain pretreated silica.

[0074] Comparative Example 1

[0075] Compared with Example 4, this comparative example does not perform the fluorene group modification treatment of silica-a and silica-b.

[0076] Comparative Example 2

[0077] Compared with Example 4, in the preparation of the fluorene-based anti-glare coating, fluorene-based modified silica-a was used to replace fluorene-based modified silica-b, that is, the particle size of the silica was all 5 μm.

[0078] Comparative Example 3

[0079] Compared with Example 4, in the preparation of the fluorene-based anti-glare coating, fluorene-based modified silica-b is used to replace fluorene-based modified silica-a, that is, the particle size of the silica is all 600 nm.

[0080] Comparative Example 4

[0081] Compared with Example 4, this comparative example adds fluorenyl-modified silica-a and fluorenyl-modified silica-b simultaneously during the prepolymerization process, and the other steps are the same.

[0082] Comparative Example 5

[0083] Compared with Example 4, this comparative example adds fluorenyl-modified silica-a and fluorenyl-modified silica-b simultaneously in the chain extension process, and the other steps are the same.

[0084] The anti-glare coatings obtained in Examples 1-6 and Comparative Examples 1-5 were coated on a transparent substrate layer (80 μm thick) made of polymethyl methacrylate by roller coating to a dry thickness of 6 μm. 2 The layer is cured by UV irradiation. The performance test is carried out as follows:

[0085] Haze:

[0086] Use NDH2000N haze meter to test. After the haze meter is blank calibrated, cut the sample into appropriate size and put it into the test chamber to measure the haze value (Haze) and total transmittance (TT).

[0087] Glossiness:

[0088] The test is carried out according to GB / T 9745-2007 "Paints and varnishes, determination of specular gloss at 20°, 60° and 85° of paint films without metallic pigments". The calibrated ETB-0686 gloss meter is used to measure 8 points at different positions of the sample coating and the average value is taken, which is recorded as the 60° gloss value of the coating.

[0089] Flash point value:

[0090] Use SMS-1000 image brightness meter, attach the sample to the image generator (resolution of 326ppi), use green light as the light source, and the flash point value tested by SMS-1000 meter is obtained by dividing the grayscale standard deviation of the filtered image by the average value. The larger the ratio, the more serious the flash point phenomenon.

[0091] Pencil hardness:

[0092] Use the Elcometer 3086 pencil hardness tester with a H-9H pencil to draw 5 lines under a load of 500g, then observe whether the film coating is scratched and judge according to the following standards:

[0093] ◎: 0-1 scratch;

[0094] ×: 2-5 scratches.

[0095] Adhesion:

[0096] Use a grid knife to gently scratch the coating, then use 3M600 to stick it evenly to the scratched part of the grid. After 5 minutes, tear off the tape, use a magnifying glass to observe the coating falling off in the grid, and judge it by the coating retention percentage, that is, if the coating falls off completely, it is judged as 0%, and if the coating is completely retained, it is judged as 100%.

[0097] Scratch resistance:

[0098] The sample coating surface was rubbed back and forth 1000 times with a load of 500g / cm2 using a reciprocating wear tester. The degree of visual damage under three-color light source:

[0099] ◎: No scars;

[0100] ○: Several minor scratches were produced;

[0101] ×: Scratches occurred on the entire surface.

[0102] crack:

[0103] According to the JIS K5600-5-1 bending test, the sample was coiled using a cylindrical mandrel and evaluated according to the following criteria based on the crack generation mode.

[0104] ◎: No cracks will occur when winding with an 8mm mandrel, and the effect is good

[0105] ×: Cracks occurred when winding with an 8 mm mandrel

[0106] Anti-glare:

[0107] A black acrylic plate was attached to the reverse side of the sample coating, and the fluorescent light from the LED light source was illuminated into the film surface to evaluate the blurriness of the reflected fluorescent light:

[0108] ◎: The outline of the fluorescent lamp is completely blurred, and the anti-glare property is good;

[0109] ○: Fluorescent light is blurry but retains its outline, and anti-glare performance is average;

[0110] ×: The outline of the fluorescent lamp can be clearly seen, and the anti-glare property is poor;

[0111] Rainbow pattern:

[0112] Cut the sample into a 10cm×10cm square and lay it flat on the LCD screen with the coating facing outward. Place the polarizer 10cm above the sample and observe the rainbow pattern of the sample through the polarizer. Evaluate according to the following standards:

[0113] ◎: No rainbow pattern

[0114] ○: Very slight rainbow pattern

[0115] ×: Visible rainbow pattern

[0116]

[0117]

[0118] The results are shown in Table 1:

[0119] It can be seen from Table 1 that the coatings prepared according to the scheme described in Examples 1-6 have appropriate haze and gloss, a total light transmittance of more than 90%, a pencil hardness of 3H, good scratch resistance, and a good appearance. No cracks, glare or rainbow patterns were observed.

[0120] Compared with Examples 1-3, Examples 4-6 add a pretreatment step of silica, which increases the number of active sites on the silica surface, improves the grafting rate, and achieves a better grafting effect, making it easier for the coating to achieve the desired hardness, adhesion, and scratch resistance.

[0121] In Comparative Example 1, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane were not used to graft and modify silica, resulting in agglomeration of silica particles and poor dispersion, which further led to a significant decrease in coating hardness and adhesion, severe scratches and cracks, poor appearance, and the appearance of obvious rainbow patterns and flashing spots.

[0122] In Comparative Example 2, silica with a particle size of 5 μm was used throughout, the haze increased slightly, and the hardness, adhesion and scratch resistance were not significantly affected. However, the anti-glare property was poor and slight rainbow patterns appeared.

[0123] In Comparative Example 3, silica with a particle size of 600 nm was used throughout, and the haze, total light transmittance, hardness, adhesion and scratch resistance were not significantly affected. However, the anti-glare property was poor and slight rainbow patterns appeared.

[0124] In Comparative Example 4, fluorenyl-modified silica-a and fluorenyl-modified silica-b are added simultaneously during the prepolymerization process. The two particle sizes of silica are unevenly distributed, and a strong cross-linking network is not formed, resulting in decreased coating density, poor hardness and adhesion, cracks, fine scratches, poor anti-glare properties, obvious rainbow patterns, and serious flash point phenomena.

[0125] In Comparative Example 5, fluorenyl-modified silica-a and fluorenyl-modified silica-b are added simultaneously during the chain extension process, the interaction force between the components is weakened, the particles are unevenly distributed, the hardness and adhesion are poor, there are cracks and fine scratches, the anti-glare property is poor, obvious rainbow patterns appear, and the flash point phenomenon is more serious.

[0126] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A method for preparing a fluorene-based anti-glare coating, characterized in that: The steps include: S1. Under a nitrogen atmosphere, 25 to 30 parts of polyisocyanate, 0.5 to 0.6 parts of fluorenyl-modified silica-a, and 150 to 200 parts of polytetrahydrofuran diol are added to a reaction container by weight, and a prepolymerization reaction is carried out at 82 to 88° C. for 2 to 2.5 hours, and then the temperature is cooled to room temperature, and 5 to 8 parts of hydroxyethyl acrylate are added, and the temperature is raised to 72 to 74° C. and the reaction is continued for 3 to 5 hours; S2, adding 2 to 6 parts of chain extender, 5 to 10 parts of methyl methacrylate, 0.2 to 0.6 parts of fluorenyl-modified silica-b, and 0.02 to 0.07 parts of azobisisobutyronitrile to the solution after the reaction in step S1, by weight, and performing a chain extension reaction at 68 to 73° C. for 2.5 to 3 hours; S3, cooling to room temperature, adding triethylamine to neutralize for 25 to 35 minutes, then adding deionized water, and high-speed shearing at 800 to 1000 rpm for 22 to 26 minutes to obtain a fluorene-containing anti-glare coating; Wherein: the fluorenyl-modified silica-a in step S1 is prepared from silica with a particle size of 1 to 5 μm, and the fluorenyl-modified silica-b in step S2 is prepared from silica with a particle size of 400 to 600 nm.

2. The method for preparing the fluorene-based anti-glare coating according to claim 1, characterized in that: The fluorene-modified silica-a is prepared by the following method: By weight, 3 to 5 parts of γ-aminopropyltriethoxysilane and 5 to 6 parts of silicon dioxide with a particle size of 1 to 5 μm are added to 80 to 100 parts of deionized water, reacted at 78 to 82° C. and 100 to 120 rpm for 1 to 2 hours, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane; By weight, 3 to 5 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene are dissolved in 80 to 100 parts of toluene solution, and 5 to 10 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica are added. Under nitrogen protection, 100 to 110 ml of a toluene solution containing 0.5 to 0.7% azobisisobutyronitrile is added at a rate of 20 ml / h. The mixture is reacted at 78 to 82° C. and 20 to 50 rpm for 13 to 15 hours. The mixture is cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorene-modified silica-a.

3. The method for preparing the fluorene-based anti-glare coating according to claim 2, characterized in that: The preparation of the fluorene-modified silica-a also includes a silica pretreatment step, which is as follows: Add silicon dioxide with a particle size of 1 to 5 μm into a sodium hydroxide solution with a pH of 10 to 12, add anhydrous ethanol thereto, alkaline-etch for 1 to 2 hours at 70 to 80° C. and 35 to 45 rpm, filter, rinse, and dry at 100 to 104° C. for 10 to 12 hours to obtain pretreated silicon dioxide.

4. The method for preparing the fluorene-based anti-glare coating according to claim 1, characterized in that: The fluorene-modified silica-b is prepared by the following method: By weight, 3 to 5 parts of γ-aminopropyltriethoxysilane and 5 to 6 parts of silicon dioxide with a particle size of 400 to 600 nm are added to 80 to 100 parts of deionized water, reacted at 78 to 82° C. and 100 to 120 rpm for 1 to 2 hours, cooled, filtered, rinsed, and dried to obtain silicon dioxide grafted with γ-aminopropyltriethoxysilane; By weight, 3 to 5 parts of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene are dissolved in 80 to 100 parts of toluene solution, and 5 to 10 parts of the above-mentioned γ-aminopropyltriethoxysilane grafted silica are added. Under nitrogen protection, 100 to 110 ml of a toluene solution containing 0.5 to 0.7% azobisisobutyronitrile is added at a rate of 20 ml / h. The mixture is reacted at 78 to 82° C. and 20 to 50 rpm for 13 to 15 hours. The mixture is cooled, filtered, rinsed and dried to obtain silica grafted with 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and γ-aminopropyltriethoxysilane, i.e., fluorene-modified silica-b.

5. The method for preparing the fluorene-based anti-glare coating according to claim 4, characterized in that: The preparation of the fluorene-modified silica-b also includes a silica pretreatment step, which is as follows: Add silicon dioxide with a particle size of 400-600 nm to a sodium hydroxide solution with a pH of 10-12, add anhydrous ethanol thereto, perform alkaline etching at 70-80° C. and 35-45 rpm for 1-2 hours, filter, rinse, and dry at 100-104° C. for 10-12 hours to obtain pretreated silicon dioxide.

6. The method for preparing the fluorene-based anti-glare coating according to claim 1, characterized in that: In step S1, the polyisocyanate is selected from one or more of toluene diisocyanate, diphenylmethane diisocyanate, and isophorone diisocyanate.

7. The method for preparing the fluorene-based anti-glare coating according to claim 1, characterized in that: In step S2, the chain extender is selected from one or more of 1,4-butanediol, ethylene glycol, propylene glycol, and 1,4-cyclohexanediol.

8. A fluorene-based anti-glare coating, characterized in that: The fluorene-based anti-glare coating is prepared by the method described in any one of claims 1-7.

9. An anti-glare film, characterized in that: The anti-glare film comprises a film layer prepared from the fluorene-containing anti-glare coating according to claim 8.

10. A polarizer, characterized in that: The polarizer includes the anti-glare film according to claim 9.

Citation Information

Patent Citations

  • Polyester film

    CN107267079A

  • Wear-resistant and impact-resistant car lamp outer lampshade and car lamp prepared from same

    CN114963122A

  • Anti-dazzle liquid, anti-dazzle film, preparation method of anti-dazzle film and polaroid

    CN115491119A

  • Anti-glare film and polarizer with the same

    US20210255366A1