Environment-friendly corrugated board bonding glue and preparation process thereof

By oxidizing starch twice and grafting modification, the problem of insufficient bonding of starch adhesive was solved, and environmentally friendly corrugated cardboard adhesive with high bond strength and anti-mold and anti-corrosion was prepared, which improved corrugated cardboard adhesion properties.

CN118879246APending Publication Date: 2024-11-01GUANGDONG JIALIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411108251.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Starch adhesives have limited their development in corrugated cardboard bonding applications due to poor adhesion, low solid content and short application period.

Method used

Through two oxidation treatments, the hydroxymethyl group is oxidized to carboxyl groups and reacts with fibers to improve bonding strength, and enhance bonding performance through monomer graft modification to prepare environmentally friendly corrugated cardboard adhesive.

Benefits of technology

It significantly improves the bonding strength and stability of the adhesive, and also has anti-mold and anti-corrosion effects, improving the bonding performance of corrugated cardboard.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to environment-friendly corrugated board bonding glue and a preparation process thereof, and belongs to the technical field of bonding glue. The invention discloses a preparation process of environment-friendly corrugated board bonding glue, which specifically comprises the following steps: (1) mixing starch and distilled water to prepare a mixed solution, and adding an oxidizing agent a for primary oxidation; (2) washing and drying, and adding sodium thiosulfate for secondary oxidation; and (3) adding a monomer and an initiator into the oxidized starch to carry out graft copolymerization reaction, and cooling to obtain the environment-friendly corrugated board bonding glue. According to the invention, through twice oxidation, hydroxymethyl in the starch is oxidized into carboxyl which can react with fibers, so that the bonding strength and stability of the adhesive are improved, meanwhile, part of hydroxymethyl in the starch is oxidized into aldehyde group which has mildew-proof and corrosion-proof effects, and the bonding strength of the adhesive is further improved through grafting modification with the monomer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesive glue and relates to an environmentally friendly corrugated board adhesive glue and a preparation process thereof. Background Art

[0002] With the continuous development of today's economy and the increasing demand for environmentally friendly materials, the development of green, low-cost and high-performance adhesive materials has become one of the goals pursued by people. Starch adhesives have become an ideal substitute for traditional synthetic resin adhesives due to their wide sources of raw material starch, low price, natural non-irritation and simple production process. However, due to its own structure and other reasons, starch adhesives have poor adhesion, low solid content and short application period, which have become shortcomings restricting their development. For this reason, it is necessary to study the modification of starch adhesives. Common methods include physical modification, chemical modification and biological modification. Among them, starch adhesives with different properties developed by chemical modification are more widely used. Summary of the invention

[0003] The present invention relates to an environmentally friendly corrugated board adhesive glue and a preparation process thereof, and belongs to the technical field of adhesive glue. The preparation process of the environmentally friendly corrugated board adhesive glue disclosed by the present invention comprises the following steps: (1) starch and distilled water are mixed to form a mixed solution, and an oxidant a is added to perform primary oxidation; (2) the mixture is then washed and dried, and an alkaline solution is added to perform secondary oxidation; (3) the oxidized starch is added with a monomer and an initiator to perform a graft copolymerization reaction, and the environmentally friendly corrugated board adhesive glue is obtained after cooling. In the present invention, the hydroxymethyl groups in the starch are oxidized into carboxyl groups through the secondary oxidation, which can react with fibers, thereby improving the bonding strength and stability of the adhesive. At the same time, a part of the hydroxymethyl groups in the starch are oxidized into aldehyde groups, which have mildew and antiseptic effects, and the graft modification with the monomer further improves the bonding strength of the adhesive.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A preparation process of an environmentally friendly corrugated board adhesive glue, the preparation process of the adhesive glue specifically comprises the following steps:

[0006] (1) Starch and distilled water are heated and stirred to form a mixed solution, an oxidant a is added and mixed, and then filtered, the solid is washed with distilled water and then dried in an oven to obtain primary oxidized starch;

[0007] (2) heating the primary oxidized starch and distilled water, adding an alkaline solution and stirring to form a mixture, then adding an oxidant a and stirring, and finally adding sodium thiosulfate and stirring, cooling to room temperature, filtering, washing the solid with distilled water, and drying to obtain secondary oxidized starch;

[0008] (3) ammonium persulfate, sodium bisulfite and distilled water are mixed, and secondary oxidized starch is added and stirred to form a mixed solution a;

[0009] (4) Butyl acrylate and sodium dodecyl sulfate are dissolved in distilled water, and an emulsion is obtained by stirring with a glass rod. The mixed solution a is stirred with the emulsion to obtain an environmentally friendly corrugated cardboard adhesive.

[0010] Furthermore, in the step (1), the ratio of starch, distilled water and oxidant a is 20-25 g:100-150 mL:5-10 mL, wherein the oxidant a is a sodium hypochlorite solution with a mass fraction of 3%.

[0011] Furthermore, the temperature of the heating in step (1) is 40-50°C, the time of adding the oxidant a and mixing is 2-3h, and the temperature and time of the drying are 50-60°C and 1h respectively.

[0012] Furthermore, in the step (2), the ratio of the primary oxidized starch, distilled water and alkaline solution is 20-30 g:100 mL:20-25 mL, wherein the alkaline solution refers to a sodium hydroxide solution with a mass fraction of 20%.

[0013] Furthermore, in the step (2), the ratio of the mixture, the oxidant a and the sodium thiosulfate is 300-350 mL: 5-10 mL: 0.1-0.3 g, the temperature of the heating and mixing is 50-60° C., the time of stirring to form the mixture is 30-60 min, the time of adding the oxidant a and stirring is 1 h, and the time and temperature of the drying are 30-60 min and 60° C., respectively.

[0014] Furthermore, in step (3), the mass ratio of ammonium persulfate, sodium bisulfite and distilled water is 1:1:50-60, and the mixing temperature and time are 50° C. and 10-15 min, respectively.

[0015] Furthermore, in step (4), the mass ratio of butyl acrylate, sodium lauryl sulfate and distilled water is 1-2:1:10-15.

[0016] Furthermore, in step (4), the stirring time of the glass rod is 5-10 min, and the stirring and mixing time and temperature are 2-4 h and 55° C. respectively.

[0017] Beneficial effects of the present invention:

[0018] 1. The present invention uses double oxidation to oxidize the hydroxymethyl groups in the starch into carboxyl groups, which can react with the fibers, thereby improving the bonding strength and stability of the adhesive. At the same time, a portion of the hydroxymethyl groups in the starch are oxidized into aldehyde groups, which have anti-mildew and anti-corrosion effects, and are grafted with the monomers to further improve the bonding strength of the adhesive. DETAILED DESCRIPTION

[0019] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.

[0020] Example 1

[0021] A preparation process of an environmentally friendly corrugated board adhesive glue, the preparation process of the adhesive glue specifically comprises the following steps:

[0022] (1) Starch and distilled water are heated and stirred to form a mixed solution, an oxidant a is added and mixed, and then filtered, the solid is washed with distilled water and then dried in an oven to obtain primary oxidized starch;

[0023] (2) heating the primary oxidized starch and distilled water, adding an alkaline solution and stirring to form a mixture, then adding an oxidant a and stirring, and finally adding sodium thiosulfate and stirring, cooling to room temperature, filtering, washing the solid with distilled water, and drying to obtain secondary oxidized starch;

[0024] (3) ammonium persulfate, sodium bisulfite and distilled water are mixed, and secondary oxidized starch is added and stirred to form a mixed solution a;

[0025] (4) Butyl acrylate and sodium dodecyl sulfate are dissolved in distilled water, and an emulsion is obtained by stirring with a glass rod. The mixed solution a is stirred with the emulsion to obtain an environmentally friendly corrugated cardboard adhesive.

[0026] In the step (1), the ratio of starch, distilled water and oxidant a is 20 g:100 mL:5 mL, wherein the oxidant a is a sodium hypochlorite solution with a mass fraction of 3%.

[0027] The temperature of the heating in step (1) is 40° C., the time of adding the oxidant a and mixing is 2 hours, and the temperature and time of the drying are 50° C. and 1 hour respectively.

[0028] In the step (2), the ratio of the primary oxidized starch, distilled water and alkaline solution is 20 g: 100 mL: 20 mL, wherein the alkaline solution refers to a sodium hydroxide solution with a mass fraction of 20%.

[0029] In the step (2), the ratio of the mixture, the oxidant a and the sodium thiosulfate is 300 mL:5 mL:0.1 g, the temperature of the heating and mixing is 50° C., the time of stirring to form the mixture is 30 min, the time of adding the oxidant a and stirring is 1 h, and the time and temperature of the drying are 30 min and 60° C. respectively.

[0030] In the step (3), the mass ratio of ammonium persulfate, sodium bisulfite and distilled water is 1:1:50, the mass ratio of ammonium persulfate to secondary oxidized starch is 1:12, and the mixing temperature and time are 50° C. and 10 min, respectively.

[0031] In the step (4), the mass ratio of butyl acrylate, sodium lauryl sulfate and distilled water is 1:1:10, and the volume ratio of the mixed solution a to the emulsion is 1:1.

[0032] In the step (4), the stirring time of the glass rod is 5 minutes, and the stirring and mixing time and temperature are 2 hours and 55° C. respectively.

[0033] Example 2

[0034] A preparation process of an environmentally friendly corrugated board adhesive glue, the preparation process of the adhesive glue specifically comprises the following steps:

[0035] (1) Starch and distilled water are heated and stirred to form a mixed solution, an oxidant a is added and mixed, and then filtered, the solid is washed with distilled water and then dried in an oven to obtain primary oxidized starch;

[0036] (2) heating the primary oxidized starch and distilled water, adding an alkaline solution and stirring to form a mixture, then adding an oxidant a and stirring, and finally adding sodium thiosulfate and stirring, cooling to room temperature, filtering, washing the solid with distilled water, and drying to obtain secondary oxidized starch;

[0037] (3) ammonium persulfate, sodium bisulfite and distilled water are mixed, and secondary oxidized starch is added and stirred to form a mixed solution a;

[0038] (4) Butyl acrylate and sodium dodecyl sulfate are dissolved in distilled water, and an emulsion is obtained by stirring with a glass rod. The mixed solution a is stirred with the emulsion to obtain an environmentally friendly corrugated cardboard adhesive.

[0039] In the step (1), the ratio of starch, distilled water and oxidant a is 22 g:125 mL:7 mL, wherein the oxidant a is a sodium hypochlorite solution with a mass fraction of 3%.

[0040] The temperature of the heating in step (1) is 45° C., the time of adding the oxidant a and mixing is 2.5 hours, and the temperature and time of the drying are 55° C. and 1 hour respectively.

[0041] In the step (2), the ratio of the primary oxidized starch, distilled water and alkaline solution is 25 g:100 mL:22 mL, wherein the alkaline solution refers to a sodium hydroxide solution with a mass fraction of 20%.

[0042] In the step (2), the ratio of the mixture, oxidant a and sodium thiosulfate is 325 mL:7 mL:0.2 g, the temperature of the heating and mixing is 55° C., the time of stirring to form the mixture is 45 min, the time of adding oxidant a and stirring is 1 h, and the time and temperature of the drying are 45 min and 60° C. respectively.

[0043] In the step (3), the mass ratio of ammonium persulfate, sodium bisulfite and distilled water is 1:1:55, the mass ratio of ammonium persulfate to secondary oxidized starch is 1:12, and the mixing temperature and time are 50° C. and 12.5 min, respectively.

[0044] In the step (4), the mass ratio of butyl acrylate, sodium lauryl sulfate and distilled water is 1.5:1:12.5, and the volume ratio of the mixed solution a to the emulsion is 1:1.

[0045] In step (4), the stirring time of the glass rod is 7 minutes, and the stirring and mixing time and temperature are 3 hours and 55° C. respectively.

[0046] Example 3

[0047] A preparation process of an environmentally friendly corrugated board adhesive glue, the preparation process of the adhesive glue specifically comprises the following steps:

[0048] (1) Starch and distilled water are heated and stirred to form a mixed solution, an oxidant a is added and mixed, and then filtered, the solid is washed with distilled water and then dried in an oven to obtain primary oxidized starch;

[0049] (2) heating the primary oxidized starch and distilled water, adding an alkaline solution and stirring to form a mixture, then adding an oxidant a and stirring, and finally adding sodium thiosulfate and stirring, cooling to room temperature, filtering, washing the solid with distilled water, and drying to obtain secondary oxidized starch;

[0050] (3) ammonium persulfate, sodium bisulfite and distilled water are mixed, and secondary oxidized starch is added and stirred to form a mixed solution a;

[0051] (4) Butyl acrylate and sodium dodecyl sulfate are dissolved in distilled water, and an emulsion is obtained by stirring with a glass rod. The mixed solution a is stirred with the emulsion to obtain an environmentally friendly corrugated cardboard adhesive.

[0052] In the step (1), the ratio of starch, distilled water and oxidant a is 25 g:150 mL:10 mL, wherein the oxidant a is a sodium hypochlorite solution with a mass fraction of 3%.

[0053] The heating temperature in step (1) is 50° C., the time for adding oxidant a and mixing is 3 hours, and the drying temperature and time are 60° C. and 1 hour respectively.

[0054] In the step (2), the ratio of the primary oxidized starch, distilled water and alkaline solution is 30 g:100 mL:25 mL, wherein the alkaline solution refers to a sodium hydroxide solution with a mass fraction of 20%.

[0055] In the step (2), the ratio of the mixture, the oxidant a and the sodium thiosulfate is 350 mL:10 mL:0.3 g, the temperature of the heating and mixing is 60° C., the time of stirring to form the mixture is 60 min, the time of adding the oxidant a and stirring is 1 h, and the time and temperature of the drying are 60 min and 60° C. respectively.

[0056] In the step (3), the mass ratio of ammonium persulfate, sodium bisulfite and distilled water is 1:1:60, the mass ratio of ammonium persulfate to secondary oxidized starch is 1:12, and the mixing temperature and time are 50° C. and 15 min, respectively.

[0057] In the step (4), the mass ratio of butyl acrylate, sodium lauryl sulfate and distilled water is 2:1:15, and the volume ratio of the mixed solution a to the emulsion is 1:1.

[0058] In the step (4), the stirring time of the glass rod is 10 minutes, and the stirring and mixing time and temperature are 4 hours and 55° C. respectively.

[0059] Comparative Example 1

[0060] On the basis of Example 3, a preparation process of an environmentally friendly corrugated board adhesive glue is provided, wherein the preparation process of the adhesive glue is specifically as follows:

[0061] (1) Mixing starch and distilled water at a high temperature, adding an alkaline solution and stirring to form a mixture, then adding an oxidant a and stirring, and finally adding sodium thiosulfate and stirring, cooling to room temperature, filtering, washing the solid with distilled water, and drying to obtain oxidized starch;

[0062] (2) ammonium persulfate, sodium bisulfite and distilled water are mixed, and oxidized starch is added and stirred to form a mixed solution a;

[0063] (3) Butyl acrylate and sodium dodecyl sulfate are dissolved in distilled water, and an emulsion is obtained by stirring with a glass rod. The mixed solution a is stirred with the emulsion to obtain an environmentally friendly corrugated cardboard adhesive.

[0064] In the step (1), the ratio of starch, distilled water and alkaline solution is 30 g:100 mL:25 mL, wherein the alkaline solution refers to a sodium hydroxide solution with a mass fraction of 20%.

[0065] In the step (1), the ratio of the mixture, the oxidant a and the sodium thiosulfate is 350 mL:10 mL:0.3 g, the temperature of the heating and mixing is 60° C., the time of stirring to form the mixture is 60 min, the time of adding the oxidant a and stirring is 1 h, and the time and temperature of the drying are 60 min and 60° C. respectively.

[0066] In the step (2), the mass ratio of ammonium persulfate, sodium bisulfite and distilled water is 1:1:60, the mass ratio of ammonium persulfate to oxidized starch is 1:12, and the mixing temperature and time are 50° C. and 15 min, respectively.

[0067] In the step (3), the mass ratio of butyl acrylate, sodium lauryl sulfate and distilled water is 2:1:15, and the volume ratio of the mixed solution a to the emulsion is 1:1.

[0068] In step (3), the stirring time of the glass rod is 10 minutes, and the stirring and mixing time and temperature are 4 hours and 55° C. respectively.

[0069] Comparative Example 2

[0070] On the basis of Example 3, a preparation process of an environmentally friendly corrugated board adhesive glue is provided, wherein the preparation process of the adhesive glue is specifically as follows:

[0071] (1) Starch and distilled water are heated and stirred to form a mixed solution, an oxidant a is added and mixed, and then filtered, the solid is washed with distilled water and then dried in an oven to obtain primary oxidized starch;

[0072] (2) ammonium persulfate, sodium bisulfite and distilled water are mixed, and primary oxidized starch is added and stirred to form a mixed solution a;

[0073] (3) Butyl acrylate and sodium dodecyl sulfate are dissolved in distilled water, and an emulsion is obtained by stirring with a glass rod. The mixed solution a is stirred with the emulsion to obtain an environmentally friendly corrugated cardboard adhesive.

[0074] In the step (1), the ratio of starch, distilled water and oxidant a is 25 g:150 mL:10 mL, wherein the oxidant a is a sodium hypochlorite solution with a mass fraction of 3%.

[0075] The heating temperature in step (1) is 50° C., the time for adding oxidant a and mixing is 3 hours, and the drying temperature and time are 60° C. and 1 hour respectively.

[0076] In the step (2), the mass ratio of ammonium persulfate, sodium bisulfite and distilled water is 1:1:60, the mass ratio of ammonium persulfate to primary oxidized starch is 1:12, and the mixing temperature and time are 50° C. and 15 min, respectively.

[0077] In the step (3), the mass ratio of butyl acrylate, sodium lauryl sulfate and distilled water is 2:1:15, and the volume ratio of the mixed solution a to the emulsion is 1:1.

[0078] In step (3), the stirring time of the glass rod is 10 minutes, and the stirring and mixing time and temperature are 4 hours and 55° C. respectively.

[0079] Comparative Example 3

[0080] On the basis of Example 3, a preparation process of an environmentally friendly corrugated board adhesive glue is provided, wherein the preparation process of the adhesive glue is specifically as follows:

[0081] (1) Starch and distilled water are heated and stirred to form a mixed solution, an oxidant a is added and mixed, and then filtered, the solid is washed with distilled water and then dried in an oven to obtain primary oxidized starch;

[0082] (2) The primary oxidized starch and distilled water are heated and mixed, an alkaline solution is added and stirred to form a mixture, then an oxidant a is added and stirred, and finally sodium thiosulfate is added and stirred, cooled to room temperature, filtered, the solid is washed with distilled water, and dried to obtain the secondary oxidized starch, 3 times the mass of distilled water is added, the temperature is raised to 50°C and stirred into a paste, which is the environmentally friendly corrugated cardboard adhesive glue.

[0083] In the step (1), the ratio of starch, distilled water and oxidant a is 25 g:150 mL:10 mL, wherein the oxidant a is a sodium hypochlorite solution with a mass fraction of 3%.

[0084] The heating temperature in step (1) is 50° C., the time for adding oxidant a and mixing is 3 hours, and the drying temperature and time are 60° C. and 1 hour respectively.

[0085] In the step (2), the ratio of the primary oxidized starch, distilled water and alkaline solution is 30 g:100 mL:25 mL, wherein the alkaline solution refers to a sodium hydroxide solution with a mass fraction of 20%.

[0086] In the step (2), the ratio of the mixture, the oxidant a and the sodium thiosulfate is 350 mL:10 mL:0.3 g, the temperature of the heating and mixing is 60° C., the time of stirring to form the mixture is 60 min, the time of adding the oxidant a and stirring is 1 h, and the time and temperature of the drying are 60 min and 60° C. respectively.

[0087] Comparative Example 4

[0088] On the basis of Example 3, a preparation process of an environmentally friendly corrugated board adhesive glue is provided, wherein the preparation process of the adhesive glue is specifically as follows:

[0089] (1) Starch and distilled water are heated and stirred to form a mixed solution, an oxidant a is added and mixed, and then filtered, the solid is washed with distilled water and then dried in an oven to obtain primary oxidized starch;

[0090] (2) heating the primary oxidized starch and distilled water, adding an alkaline solution and stirring to form a mixture, then adding an oxidant a and stirring, and finally adding sodium thiosulfate and stirring, cooling to room temperature, filtering, washing the solid with distilled water, and drying to obtain secondary oxidized starch;

[0091] (3) ammonium persulfate, sodium bisulfite and distilled water are mixed, and secondary oxidized starch is added and stirred to form a mixed solution a;

[0092] (4) Propylene oxide and sodium dodecyl sulfate are dissolved in distilled water, and an emulsion is obtained by stirring with a glass rod. The mixed solution a is stirred with the emulsion to obtain an environmentally friendly corrugated cardboard adhesive.

[0093] In the step (1), the ratio of starch, distilled water and oxidant a is 25 g:150 mL:10 mL, wherein the oxidant a is a sodium hypochlorite solution with a mass fraction of 3%.

[0094] The heating temperature in step (1) is 50° C., the time for adding oxidant a and mixing is 3 hours, and the drying temperature and time are 60° C. and 1 hour respectively.

[0095] In the step (2), the ratio of the primary oxidized starch, distilled water and alkaline solution is 30 g:100 mL:25 mL, wherein the alkaline solution refers to a sodium hydroxide solution with a mass fraction of 20%.

[0096] In the step (2), the ratio of the mixture, the oxidant a and the sodium thiosulfate is 350 mL:10 mL:0.3 g, the temperature of the heating and mixing is 60° C., the time of stirring to form the mixture is 60 min, the time of adding the oxidant a and stirring is 1 h, and the time and temperature of the drying are 60 min and 60° C. respectively.

[0097] In the step (3), the mass ratio of ammonium persulfate, sodium bisulfite and distilled water is 1:1:60, the mass ratio of ammonium persulfate to secondary oxidized starch is 1:12, and the mixing temperature and time are 50° C. and 15 min, respectively.

[0098] In the step (4), the mass ratio of propylene oxide, sodium lauryl sulfate and distilled water is 2:1:15, and the volume ratio of the mixed solution a to the emulsion is 1:1.

[0099] In the step (4), the stirring time of the glass rod is 10 minutes, and the stirring and mixing time and temperature are 4 hours and 55° C. respectively.

[0100] 1. Performance Testing

[0101] Bond strength: The adhesive glue prepared in Examples 1-3 and Comparative Examples 1-4 was used as a sample. The base paper was heated and sent to a single-facer to be pressed into the required fluted paper core. The paper core was coated with a thickness of 3 g / m 2 The sample is then sandwiched between the inner paper and the face paper to obtain the corrugated cardboard after drying. The corrugated cardboard is cut into 2cm×15cm strips and the paper peeling strength is measured using a WZL-300 paper tensile tester.

[0102] Anti-mildew test: The adhesives prepared in Examples 1-3 and Comparative Examples 1-4 were coated on clean glass sheets respectively, placed at room temperature, and observed for mildew after one month.

[0103] The above test results are shown in Table 1:

[0104] Table 1 Test results

[0105] Sample Peel strength kN / m Tensile strength / MPa Mildew resistance test Example 1 0.394 13.68 No mold Example 2 0.406 13.60 No mold Example 3 0.390 13.62 No mold Comparative Example 1 0.275 10.51 No mold Comparative Example 2 0.287 10.68 get mouldy Comparative Example 3 0.254 11.03 No mold Comparative Example 4 0.326 11.54 No mold

[0106] As can be seen from Table 1, the peel strength of Examples 1-3 is greater than that of Comparative Examples 1-4, and the tensile strength is also greater than that of Comparative Examples 1-4. In addition, mold occurs in Comparative Example 2. The starch in Comparative Example 1 was not oxidized once, and a large number of hydroxymethyl groups still existed in the starch, which affected the bonding strength of the adhesive. Comparative Example 2 was not oxidized twice, and the bonding strength of the adhesive was also reduced. In addition, mold occurred because the number of aldehyde groups oxidized was reduced. In Comparative Example 3, the oxidized starch was not further grafted and modified, and its bonding strength was worse than that of the examples. In Comparative Example 4, the butyl acrylate monomer was replaced with propylene oxide monomer, and its bonding effect was reduced.

[0107] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A preparation process of an environmentally friendly corrugated board adhesive, characterized in that: The preparation process of the adhesive glue is specifically as follows: (1) Starch and distilled water are heated and stirred to form a mixed solution, an oxidant a is added and mixed, and then filtered, the solid is washed with distilled water and then dried in an oven to obtain primary oxidized starch; (2) heating the primary oxidized starch and distilled water, adding an alkaline solution and stirring to form a mixture, then adding an oxidant a and stirring, and finally adding sodium thiosulfate and stirring, cooling to room temperature, filtering, washing the solid with distilled water, and drying to obtain secondary oxidized starch; (3) ammonium persulfate, sodium bisulfite and distilled water are mixed, and secondary oxidized starch is added and stirred to form a mixed solution a; (4) Butyl acrylate and sodium dodecyl sulfate are dissolved in distilled water, and an emulsion is obtained by stirring with a glass rod. The mixed solution a is stirred with the emulsion to obtain an environmentally friendly corrugated cardboard adhesive.

2. The preparation process of an environmentally friendly corrugated board adhesive according to claim 1, characterized in that: In the step (1), the ratio of starch, distilled water and oxidant a is 20-25 g:100-150 mL:5-10 mL, wherein the oxidant a is a sodium hypochlorite solution with a mass fraction of 3%.

3. The preparation process of an environmentally friendly corrugated board adhesive according to claim 1, characterized in that: The temperature of the heating in step (1) is 40-50° C., the time of adding the oxidant a and mixing is 2-3 hours, and the temperature and time of the drying are 50-60° C. and 1 hour respectively.

4. The process for preparing an environmentally friendly corrugated board adhesive according to claim 1, characterized in that: In the step (2), the ratio of the primary oxidized starch, distilled water and alkaline solution is 20-30 g:100 mL:20-25 mL, wherein the alkaline solution refers to a sodium hydroxide solution with a mass fraction of 20%.

5. The process for preparing an environmentally friendly corrugated board adhesive according to claim 1, characterized in that: In the step (2), the ratio of the mixture, the oxidant a and the sodium thiosulfate is 300-350 mL: 5-10 mL: 0.1-0.3 g, the temperature of the heating and mixing is 50-60° C., the time of stirring to form the mixture is 30-60 min, the time of adding the oxidant a and stirring is 1 h, and the time and temperature of the drying are 30-60 min and 60° C. respectively.

6. The process for preparing an environmentally friendly corrugated board adhesive according to claim 1, characterized in that: In the step (3), the mass ratio of ammonium persulfate, sodium bisulfite and distilled water is 1:1:50-60, and the mixing temperature and time are 50° C. and 10-15 min, respectively.

7. The process for preparing an environmentally friendly corrugated board adhesive according to claim 1, characterized in that: In the step (4), the mass ratio of butyl acrylate, sodium lauryl sulfate and distilled water is 1-2:1:10-15.

8. The process for preparing an environmentally friendly corrugated board adhesive according to claim 1, characterized in that: In the step (4), the stirring time of the glass rod is 5-10 min, and the stirring and mixing time and temperature are 2-4 h and 55° C. respectively.