Method for improving segregation of 20CrMnTiH square frame
By optimizing the steelmaking and rolling process in 20CrMnTiH alloy, the serious segregation problem in the alloy is solved, the segregation index is reduced, the performance and stability of the material are improved, and the quality of the finished products is achieved.
Patent Information
- Application Number
- CN202410964837.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art has serious segregation problems in 20CrMnTiH alloys, which affect the physical and mechanical properties of the materials, especially in the heating and shearing process, which leads to the occurrence of microcracks and macrocracks, and the existing methods are difficult to effectively control segregation.
By optimizing the steelmaking and rolling process, including setting a vacuum time of 12-15 minutes and a soft blow time of 16-20 minutes in the RH furnace, precise control of chemical composition, low-pull speed and weak cooling process and 13 passes of reversible The rolling process controls the rolling procedures and parameters of the billet opener to reduce segregation.
The 20CrMnTiH box segregation index was significantly reduced from 1.29 to 1.10, which improved the internal quality and performance stability of the material, reduced cracks and brittle problems, and improved the strength and corrosion resistance of the finished product.
Smart Images

Figure CN118879984A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel rolling and relates to a method for improving 20CrMnTiH frame segregation. Background Art
[0002] Segregation of 20CrMnTiH refers to the phenomenon that the chemical composition of the newly formed solid phase and the surrounding liquid phase is uneven due to the redistribution of solute elements during the solidification process of the alloy. Macrosegregation (regional segregation): The uneven distribution of solute elements in a range larger than the grain size. Large-size macrosegregation will seriously affect the physical and mechanical properties of the material. Microsegregation: The uneven distribution of chemical composition in the microstructure, usually including dendrite segregation, cellular segregation, grain boundary segregation, etc. Although the size range is small, it will also affect the performance of the material, such as corrosion resistance. Segregation may prevent the material from achieving the expected strength, toughness, corrosion resistance, etc., and will also cause quality problems in the material, such as cracks and increased brittleness. As an alloy structural steel, 20CrMnTiH's chemical composition includes elements such as carbon, silicon, manganese, chromium and titanium. The precise ratio of these elements gives 20CrMnTiH excellent physical properties. However, during the solidification of the alloy, segregation may occur due to the redistribution of solute elements. In the heating shearing process of 20CrMnTiH, if the heating is not sufficient, the segregation in the microstructure is serious, which may lead to the formation of martensite and bainite structures in the segregation zone. These structures are prone to microcracks during low-temperature shearing, which then develop into macrocracks. At the same time, rolling will also affect the segregation of 20CrMnTiH. Figure 1 The 20CrMnTiH square frame segregation object of the prior art has not been improved, and the segregation index is 1.29.
[0003] Chinese invention patent CN202111357579.3 discloses an RH refining process for suppressing the formation of large-sized TiN-containing composite inclusions in 20CrMnTi steel. In view of the segregation problem caused by TiN composite inclusions in 20CrMnTiH steel, the RH method (a steel liquid vacuum treatment technology) is used to suppress the formation of such inclusions. By controlling the formation of MgO-Al2O3-TiOx-type oxides during smelting and solidification, the heterogeneous nucleation rate of TiN inclusions is reduced, thereby solving the problem of large-sized composite TiN inclusions and TiN aggregation. However, although the invention has a certain effect on suppressing large-sized composite inclusions by precisely controlling residual elements, it lacks the effect of controlling segregation. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art, provide a method for improving the square segregation of 20CrMnTiH, improve the square segregation of 20CrMnTiH continuous casting billets and 20CrMnTiH rolled billets, and improve the product quality of 20CrMnTiH finished products.
[0005] The technical solution adopted by the present invention to solve the technical problem is a method for improving the square frame segregation of 20CrMnTiH. The key technical parameters are as follows:
[0006] (1) The vacuum time of RH furnace is 12-15 minutes, and the soft blowing time is 16-20 minutes;
[0007] (2) Control the C content of 20CrMnTiH steel to 0.19-0.20%, Si content to 0.18-0.22%, Mn content to 1.08-1.11%, P content to ≤0.013%, S content to 0.015-0.025%, Cr content to 1.25-1.28%, and Ti content to 0.05-0.06%;
[0008] (3) The crystallizer electromagnetic stirring current is 150-170A, the frequency is 2.5-3Hz, the end electromagnetic stirring current is 250-300A, the frequency is 8-10Hz; the low-speed weak cooling process is adopted, the casting speed is 0.45-0.48m / min, and the secondary cooling water volume is 0.22-0.24L / kg;
[0009] (4) The slab mill adopts 13-pass reversible rolling to control whether the steel is turned and the reduction amount, and the reduction amount is ±10 mm. The rolling program of the slab mill is shown in Table 1. In this step, the reduction amount of the pass is increased in a targeted manner according to whether the steel is turned to reduce the degree of segregation.
[0010] Furthermore, in step (4), the groove depth, height, width and aspect ratio are controlled; the rolling program of the slab mill is shown in Table 2. The height deviation is ±10 mm, and the reduction is ±10 mm.
[0011] Table 1 13-pass rolling program of billet mill
[0012]
[0013] Table 2 13-pass rolling program of the billet mill
[0014]
[0015] The method for improving the square frame segregation of 20CrMnTiH of the present invention improves the square frame segregation of 20CrMnTiH continuous casting billet and 20CrMnTiH rolled billet by optimizing the steelmaking process and the rolling process, thereby improving the internal quality of the finished product.
[0016] The design improvement principle and beneficial effects of the present invention are as follows:
[0017] 1. During the vacuum maintenance process of the RH furnace, the gas in the furnace is extracted through a vacuum pump, which can effectively remove oxygen and other impurities in the molten steel. This purification process is crucial to improving the quality and internal quality of steel. Before the molten steel is cast, a certain amount of inert gas is used to continuously agitate the molten steel from the bottom of the ladle. This process is called soft blowing. Studies have shown that the vacuum maintenance time of the RH furnace is 12-15 minutes, the soft blowing time is 16-20 minutes, the molten steel has good castability, the stopper rod stroke and the crystallizer liquid level control are stable; it can improve the composition stability of the continuous casting billet and reduce the segregation index.
[0018] In the steelmaking process of RH furnace (vacuum circulation degassing furnace), the vacuum holding time and soft blowing time have an important influence on the castability of molten steel. In the actual operation of RH furnace, the setting of vacuum holding time and soft blowing time should be comprehensively considered according to factors such as steel type, molten steel quality requirements and production efficiency.
[0019] Maintaining the vacuum for too long: 1. Maintaining the vacuum for a long time will increase energy consumption and raise production costs; 2. Long-term operation of key equipment such as vacuum pumps will accelerate wear and affect equipment life; 3. Although long-term vacuum treatment helps to further remove gases and inclusions in the steel, it may also cause excessive oxidation of the molten steel or volatilization of alloy elements, affecting the quality of the molten steel.
[0020] The vacuum time is too short: 1. Short-term vacuum treatment may not effectively remove gases in the molten steel, such as hydrogen and nitrogen, which will affect the purity and performance of the molten steel. 2. Insufficient removal of inclusions may lead to poor castability of the molten steel, affecting the subsequent casting process.
[0021] Soft blowing time is too long: 1. Long soft blowing time will cause the temperature of molten steel to drop significantly, which will have an adverse effect on subsequent pouring, such as increasing the difficulty of pouring and affecting the quality of the ingot. 2. Too long soft blowing time will reduce production efficiency and increase production cycle.
[0022] Soft blowing time is too short: 1. The main purpose of soft blowing is to promote the floating and removal of inclusions through argon stirring. If the soft blowing time is insufficient, the inclusions may not be fully floated and removed, thus affecting the castability of the molten steel and the quality of the ingot. 2. Short-term soft blowing may not make the molten steel temperature, composition and inclusion distribution reach an ideal uniform state.
[0023] 2. Compared with the national standard content of each element (C content is 0.17-0.23%, Si content is 0.17-0.37%, Mn content is 0.80-1.20%, P content is ≤0.03%, S content is ≤0.035%, Cr content is 1.10-1.45%, Ti content is 0.04-0.10%), the method of improving the segregation of 20CrMnTiH frame of the present invention further accurately controls the content of each element. Carbon (C) content: reduced from 0.17-0.23% in the national standard to 0.19-0.20%; accurate control of carbon content has a direct impact on the hardness, strength and hardenability of steel, helps to reduce segregation, and improves the uniformity and performance stability of steel. Silicon (Si) content: reduced from 0.17-0.37% in the national standard to 0.18-0.22%; Silicon improves the strength and hardness of steel, and also helps to improve the corrosion resistance of steel; reducing the range of silicon content can further optimize the performance of steel. Manganese (Mn) content: reduced from 0.80-1.20% in the national standard to 1.08-1.11%; Manganese is an important alloying element in steel, and has a significant effect on improving the strength, hardness and hardenability of steel; precise control of manganese content helps to reduce segregation and improve the performance of steel. Phosphorus (P) content: The national standard requires a phosphorus content of ≤0.03%, while the phosphorus content is controlled to ≤0.013% in the present invention; Phosphorus is a harmful element in steel, and too much phosphorus will reduce the toughness and weldability of steel; reducing the phosphorus content can improve the toughness and machinability of steel. Sulfur (S) content: The national standard requires a sulfur content of ≤0.035%, while the sulfur content in the present invention is controlled to be 0.015-0.025%; Sulfur is also a harmful element in steel. Excessive sulfur can cause hot brittleness of steel, but in certain specific applications, steel needs to have a certain sulfur content to meet its specific performance requirements; 20CrMnTiH needs to have a certain work hardening ability or wear resistance while maintaining a certain toughness and strength. In this case, appropriately increasing the sulfur content (but still within a controllable range) helps to achieve these performance requirements; Accurately controlling the sulfur content can improve the hot working performance and toughness of steel. Chromium (Cr) content: Reduced from 1.10-1.45% in the national standard to 1.25-1.28%; Chromium is an important alloying element in steel, which plays an important role in improving the hardness, wear resistance and corrosion resistance of steel; Accurately controlling the chromium content helps to optimize the performance of steel. Titanium (Ti) content: reduced from 0.04-0.10% in the national standard to 0.05-0.06%. Titanium can be used as an element to refine grains in steel, thereby improving the strength and toughness of steel. Narrowing the range of titanium content helps to more accurately control the grain size and performance of steel.
[0024] 3. When the electromagnetic stirring intensity of the continuous casting billet is too high, the subcutaneous solute elements are washed away, forming negative segregation. The equiaxed crystal area is carbon negative segregation, and the columnar crystal area is carbon positive segregation. The difference is large, and the ingot segregation is inherited to the rolled material. By adjusting the continuous casting process parameters, reducing the electromagnetic stirring intensity of the crystallizer and increasing the specific water content, the columnar crystal area is increased, the equiaxed crystal area is reduced, the subcutaneous negative segregation is reduced, and the segregation of the continuous casting billet is reduced. By changing the specific water content and electromagnetic stirring intensity and controlling the equiaxed crystal ratio, the ingot segregation of the rolled material can be controlled and the cross-sectional carbon distribution tends to be uniform. The crystallizer electromagnetic stirring current is 150-170A and the frequency is 2.5-3Hz, the end electromagnetic stirring current is 250-300A and the frequency is 8-10Hz; the casting machine pulling speed is 0.45-0.48m / min, the secondary cooling water volume is 0.22-0.24L / kg, and the macro-segregation of the carbon content produced is better, and the segregation index is close to 1, which is 1.10-1.12.
[0025] 4. The ingot opening machine is optimized from 11 passes to 13 passes. Through targeted steel turning and increased reduction, the uneven deformation during the rolling process can change the shape of the ingot segregation. 13 passes are used for rolling, and all odd passes except the 13th pass are steel turning passes, and even passes are not steel turning. The design that is conducive to steel turning passes (odd passes) helps the steel to obtain more uniform heating and deformation during the rolling process. This uniformity can reduce the temperature gradient and stress concentration inside the steel, thereby reducing the occurrence of segregation; through the steel turning operation of odd passes, the flow direction and speed of the steel during the rolling process can be more effectively controlled. This control can ensure that each part of the steel is subjected to the same or similar stress and deformation during rolling, thereby reducing the possibility of segregation; the design of no steel turning in even passes can maintain the stable forward direction of the steel during the rolling process and avoid unnecessary twisting or bending during the rolling process. This stable rolling path helps maintain the uniformity of the internal structure of the steel and reduce segregation; 13-pass rolling provides more rolling steps and control points compared to traditional rolling methods. This helps to more accurately control the size and shape of the steel, thereby reducing segregation problems caused by dimensional deviations or shape defects. The specific values are shown in Table 1. The first 1-4 passes are rolled in 1 hole respectively. In the initial stage, the steel is rolled in a smaller hole position, which helps to initially shape and homogenize the internal structure of the steel; 5-8 passes are rolled in 2 holes respectively. As the steel gradually deforms, it is transferred to a slightly smaller hole position for rolling, which helps to further refine the organizational structure of the steel and reduce the possibility of segregation. 9-10 passes are 3 / 2 hole alternating rolling. At this stage, the steel is rolled alternately between 3 holes and 2 holes. This alternating rolling may help break the segregation structure that may be formed inside the steel, and reduce segregation by changing the rolling path and stress distribution. 11-13 passes are rolled in 4 holes. In the final stage of rolling, the steel is rolled in the smallest hole position, which helps to finalize the size and shape of the steel and further improve the uniformity of the internal structure of the steel. Through 13 passes of rolling, the steel undergoes multiple deformation and recrystallization processes, which helps to break and reduce the segregation structure inside the steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the actual picture of the 20CrMnTiH square frame segregation before the prior art is improved, and the segregation index is 1.29;
[0027] Figure 2 This is a physical picture of the 20CrMnTiH product after rolling in the embodiment of the present invention, with a segregation index of 1.10;
[0028] Figure 3-15 They are respectively diagrams showing the size, characteristic point positions, deformation and segregation zone changes of 20CrMnTiH rolled piece after the 1st to 13th rolling passes in the embodiment of the present invention. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0030] Example 1
[0031] The key technical parameters of the method for improving the 20CrMnTiH frame segregation in this embodiment are as follows:
[0032] (1) The vacuum time of RH furnace is 12 minutes, and the soft blowing time is 16-20 minutes;
[0033] (2) Control the C content of 20CrMnTiH steel to 0.20%, Si content to 0.21%, Mn content to 1.10%, P content to 0.009%, S content to 0.021%, Cr content to 1.27%, and Ti content to 0.052%;
[0034] (3) The crystallizer electromagnetic stirring current is 150-170A, the frequency is 2.5-3Hz, the end electromagnetic stirring current is 250-300A, the frequency is 8-10Hz; the low-speed weak cooling process is adopted, the casting speed is 0.45-0.48m / min, and the secondary cooling water volume is 0.22-0.24L / kg;
[0035] (4) The slab mill adopts 13-pass reversible rolling to control whether the steel is turned and the amount of reduction, and to control the groove depth, height, width and aspect ratio; the rolling program of the slab mill is shown in Table 2. The height deviation is ±2mm, and the reduction is ±2mm. In this step, combined with whether the steel is turned, the reduction of this pass is targeted to reduce the degree of segregation.
[0036] Table 3 Example of slab mill 13-pass rolling program
[0037]
[0038] Figure 3-15 The following are the changes in the size, characteristic point positions, deformation and segregation zones of the 20CrMnTiH rolled piece after the 1st to 13th rolling passes of the embodiment of the present invention, from which we can see the microscopic changes after each rolling pass.
[0039] The method for improving the square frame segregation of 20CrMnTiH of the present invention improves the square frame segregation of 20CrMnTiH continuous casting billet and 20CrMnTiH rolled billet by optimizing the steelmaking process and the rolling process, thereby improving the internal quality of the finished product.
[0040] In this embodiment, the raw material ingot before rolling was tested and no obvious cracks or shrinkage defects were found, but there was box segregation and the aspect ratio was relatively large, which was 1.52.
[0041] After rolling, the square segregation aspect ratio of the obtained 20CrMnTiH product in this embodiment is 1.10. Figure 2 shown.
[0042] The performance test of the 20CrMnTiH product obtained in this embodiment is as follows:
[0043] 1. Low-magnification test results
[0044] Two low-magnification specimens were taken from each rolled round steel for testing. The low-magnification test results were normal, and the length-to-width ratio of the square segregation was 1.10.
[0045] Table 4
[0046]
[0047] 2. Gas inspection
[0048] The gas content was tested by furnace, and the test results all met the requirements. The specific test results are as follows:
[0049] Table 5
[0050]
[0051] 3. High magnification inspection
[0052] 3.1 Inclusion Detection
[0053] The non-metallic inclusions of steel are tested according to GB / T10561 A method. The sulfide inclusions are under normal control and meet the requirements. The inclusion requirements and rating results are as follows:
[0054]
[0055] Table 6 Non-metallic inclusions (grade)
[0056] 3.2 Austenite grain size
[0057] Steel samples were tested according to the simulated carburizing method in GB / T6394. The steel samples were heated to 930°C, kept warm for 8 hours, and then water-cooled. The austenite grain rating result was 8-8.5, meeting the requirement of being greater than 6.
[0058] 3.3 Banded tissue
[0059] The metallographic and banded structures are tested according to GB / T13299. The test standards and results are as follows:
[0060] Table 7
[0061] Brand Specification Banded Organization Level Example 20CrMnTiSH4 φ140mm 1.5 / 1.5
[0062] 3.4 End hardenability
[0063] The hardenability test results all meet the requirements, and the test results are as follows:
[0064] Table 820CrMnTiSH4 end quenching test results
[0065]
[0066]
[0067] 3.5 Mechanical properties
[0068] The sample size, heat treatment system, etc. should comply with the requirements of GB / T 3077 standard. The test results all meet the requirements. The results are shown in the following table:
[0069] Table 920CrMnTiSH4 mechanical properties test results
[0070]
[0071] 3.6 Carbon content macrosegregation detection
[0072] Table 10
[0073]
[0074] It can be seen that the low-magnification structure, banded structure, inclusion content, gas content, and mechanical property test of the finished product of this embodiment all meet the requirements. The rolling production adopts 13 passes of pressing, and the segregation aspect ratio of the rolled round steel frame is 1.10-1.12, which is significantly lower than the segregation aspect ratio of 1.28 of the prior art 11 passes of rolling frame.
[0075] Comparative Example 1
[0076] In this comparative example, except that the steel was not turned over in the third pass, other operations and parameters were the same as those in Example 1. The aspect ratio of the obtained 20CrMnTiH square frame segregation was 1.16.
[0077] Comparative Example 2
[0078] In this comparative example, except that the steel was not turned over in the 7th pass, other operations and parameters were the same as those in Example 1. The aspect ratio of the obtained 20CrMnTiH square frame segregation was 1.17.
[0079] Comparative Example 3
[0080] In this comparative example, except that the third pass reduction was 20 mm, other operations and parameters were the same as those in Example 1. The aspect ratio of the obtained 20CrMnTiH square frame segregation was 1.18.
[0081] Comparative Example 4
[0082] In this comparative example, except that the eighth pass reduction was 50 mm, other operations and parameters were the same as those in Example 1. The obtained 20CrMnTiH square frame segregation aspect ratio was 1.20.
Claims
1. A method for improving 20CrMnTiH frame segregation, characterized in that: The key technical parameters are as follows: (1) The vacuum time of RH furnace is 12-15 minutes, and the soft blowing time is 16-20 minutes; (2) Control the C content of 20CrMnTiH steel to 0.19-0.20%, Si content to 0.18-0.22%, Mn content to 1.08-1.11%, P content to ≤0.013%, S content to 0.015-0.025%, Cr content to 1.25-1.28%, and Ti content to 0.05-0.06%; (3) The crystallizer electromagnetic stirring current is 150-170A, the frequency is 2.5-3Hz, the end electromagnetic stirring current is 250-300A, the frequency is 8-10Hz; the low-speed weak cooling process is adopted, the casting speed is 0.45-0.48m / min, and the secondary cooling water volume is 0.22-0.24L / kg; (4) The slab mill adopts 13-pass reversible rolling to control whether to turn the steel and the amount of reduction. The rolling program of the slab mill is shown in Table 1; Table 1 13-pass rolling program of billet mill 2. The method for improving the frame segregation of 20CrMnTiH according to claim 1, characterized in that: In step (4), the groove depth, height, width and aspect ratio are controlled; the rolling program of the slab mill is shown in Table 2; Table 2 13-pass rolling program of the billet mill 3. The method for improving 20CrMnTiH frame segregation according to claim 1 or 2, characterized in that: In step (4), the pressing amount is ±10 mm.
4. The method for improving 20CrMnTiH frame segregation according to claim 2, characterized in that: In step (4), the height deviation is ±10 mm.
Citation Information
Patent Citations
RH (Ruhrstahl Heraeus) refining process for inhibiting 20CrMnTi steel from generating large-size TiN-containing composite inclusions
CN114231698A