Method for pretreating and recycling electroplating sludge through synergistic biological oxidation
Through the coordinated biological oxidation pretreatment method, the pH value of the copper and zinc hydroxide in the electroplating sludge is neutralized and the pH value of the biological oxidation solution is recovered in combination with the ion exchange resin, which solves the pH value drop and resources in electroplating sludge treatment. The problem of poor purification effect has achieved efficient resource utilization and environmentally friendly metal recycling.
Patent Information
- Application Number
- CN202410981995.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-22
AI Technical Summary
During the electroplating sludge treatment, the decrease in the pH value of the biological oxidation liquid leads to adverse bacterial growth, affecting the production efficiency of gold-raising, and the existing technology has no significant resource effect, is unfriendly in the environment, and has a large carbon emissions.
The electroplating sludge and biological oxidation pretreatment method are adopted to coordinate the treatment of electroplating sludge and biological oxidation solution. The copper and zinc hydroxide in the sludge are used to neutralize the pH of the oxide solution, and the valuable metal elements are recovered in combination with ion exchange resin to achieve resource utilization. .
It effectively improves the production efficiency of bio-oxidation pretreatment, realizes the resource utilization of valuable metals, reduces the consumption of acid or ammonia, reduces carbon emissions, and improves the operating environment.
Smart Images

Figure BDA0004956350160000031 
Figure HDA0004956350170000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mineral processing engineering, and in particular relates to a method for pre-treating resource-based electroplating sludge by coordinated biological oxidation. Background Art
[0002] Electroplating sludge is the precipitate formed after treating electroplating wastewater. It is mainly composed of hydroxides and carbonates of metals such as copper and zinc. It has the characteristics of high water content, high thermal stability of heavy metal components and easy migration. It is very easy to cause secondary pollution and is a hazardous waste. In view of the decrease in pH of the biological oxidation liquid, the method of adding CaO for neutralization is often used on site. If not treated, the biological oxidation liquid will not be able to meet or even hinder on-site production and become waste liquid. The properties of electroplating sludge vary with the production process and treatment process of the electroplating manufacturer. There are challenges in harmless treatment and separation and comprehensive utilization. In recent years, the treatment of electroplating sludge at home and abroad has focused on the following aspects: 1. Solidification and stabilization technology, such as patent CN03126608.8 "Method for comprehensive utilization, stabilization and solidification of industrial waste residues for electroplating sludge" 2. Acid leaching method, such as patent CN202110504703.8 "A method for resource recovery of high-content copper and nickel electroplating sludge" 3. Ammonia leaching method, such as patent CN202110504703.8 "A method for resource recovery of high-content copper and nickel electroplating sludge" 3. Ammonia leaching method, such as patent CN20211 1175147.0 "System and process for recovering copper, nickel, zinc, chromium and iron from electroplating sludge or other multi-metal mixtures" 4. Bioleaching method, such as patent CN202310639330.4 "A method for electro-chemical enhanced bioleaching of heavy metals in electroplating sludge" 5. Smelting method, such as patent CN202310993004.3 "A method for recovering valuable metals in electroplating sludge" 6. Preparation of ceramic materials, such as patent CN201610417252.3 "Electroplating sludge ceramic aggregate and its manufacturing method".
[0003] Electroplating sludge can be divided into two categories: mixed sludge and differentiated sludge. Although traditional solidification and stabilization technologies and the preparation of ceramic materials can absorb a considerable amount of electroplating sludge and eliminate material pollution problems, they do not actually fully utilize the valuable elements in the sludge, and the resource utilization effect is not significant; acid leaching and ammonia leaching are typical technologies for recovering valuable metals in electroplating sludge, but the consumption of acid or ammonia in the process is large, and the operating environment is not friendly; the smelting method uses coal and coke as fuel and reducing materials to recover valuable elements, but there are large carbon emissions in the process, and the smelting furnace temperature is mostly above 1000°C, and the operating environment is relatively harsh.
[0004] Biological oxidation pretreatment is aimed at difficult-to-treat gold ores. Microorganisms such as Thiobacillus ferrooxidans are used to oxidize gold-wrapped pyrite, arsenopyrite and other components under acidic conditions to expose the gold. Most biological oxidation reactions are acid-producing processes, which will cause the pH value of the solution to decrease, generally between 1.2 and 1.8, while the pH value suitable for bacterial growth is 1.8 to 2.5. Obviously, the biological oxidation liquid environment is not conducive to bacterial growth and metabolism, and ultimately affects the gold extraction production efficiency. Summary of the invention
[0005] In view of the problems existing in the background technology, the present invention provides a method for synergistic bio-oxidation pretreatment of resource-based electroplating sludge, which combines the bio-oxidation liquid and electroplating sludge in the bio-oxidation process of difficult-to-treat gold mines, wherein the acidic bio-oxidation liquid can be used as a leaching liquid for acid leaching of electroplating sludge, thereby effectively utilizing the valuable metal elements in the electroplating sludge; and during the process, the copper and zinc hydroxides and carbonates in the electroplating sludge can effectively neutralize the pH of the oxidation liquid, enhance bacterial activity, and improve the production efficiency of bio-oxidation pretreatment, thereby truly realizing "waste treatment with waste".
[0006] The present invention provides a method for pre-treating resource-based electroplating sludge by coordinated biological oxidation, and the specific steps are as follows:
[0007] Step 1: Slurry treatment: Slurry treatment refers to the operation of adding solvent to solid particles and mixing the two thoroughly, which can further disperse the electroplating sludge. The electroplating sludge and water are fed into the slurry machine for slurry treatment.
[0008] Step 2, synergistic treatment: This step cooperates with the biological oxidation pretreatment to obtain the valuable metal elements in the electroplating sludge. In addition, the electroplating sludge is mostly alkaline oxides of valuable metal elements, which can be used as neutralizers for the biological oxidation liquid. The electroplating sludge after slurry treatment is fed into the biological oxidation liquid, mixed and reacted to obtain a synergistic treatment product.
[0009] Step 3: Filtration: The co-processed product obtained in step 2 is subjected to solid-liquid separation to obtain a filtrate and a filter residue, respectively.
[0010] Step 4, ion exchange process: use ion exchange resin to remove the valuable elements in the filtrate obtained in step 3; feed the filtrate obtained in step 3 into the cation exchange resin from top to bottom, and the valuable metal ions in the filtrate will be adsorbed into the cation exchange resin.
[0011] Step 5: Desorption: Treat the cation exchange resin with an acid solution to obtain an enriched solution containing copper and zinc ions.
[0012] Furthermore, in the step 1, the ratio of electroplating sludge to water is, by mass ratio, (1-1.8):1, and the stirring speed during slurry treatment is 300-500 r / min.
[0013] Furthermore, in step 2, the valuable element is selected from one or more of copper and zinc.
[0014] Furthermore, in step 2, the biological oxidation liquid is a biological oxidation liquid produced during the biological oxidation process of refractory gold ore.
[0015] Furthermore, in the step 2, the ratio of the electroplating sludge after slurry treatment to the biological oxidation liquid is, by volume, 1:(2-3); the coordinated treatment temperature is 25-30° C., and the coordinated treatment time is 15-20 hours.
[0016] Furthermore, in step three, the filtrate contains valuable metal elements in the electroplating sludge, and the filter residue contains the refractory gold ore and suspended matter that is insoluble in acid after being treated with bacteria in the biological oxidation liquid.
[0017] Furthermore, in step 4, during the ion exchange process, the filtrate height needs to be always higher than the cation exchange resin layer. When the effluent concentration of the cation exchange resin reaches the flow point, the filtrate feeding is stopped and the ion exchange is terminated.
[0018] Furthermore, in step 5, the acid solution is selected from inorganic acids, specifically including hydrochloric acid, sulfuric acid, and nitric acid, and the concentration is 5% to 20% by mass.
[0019] Beneficial effects of the present invention:
[0020] Advantage 1 of the present invention is that the electroplating sludge is treated by a coordinated biological oxidation pretreatment process, and valuable elements such as copper and zinc therein are recovered to achieve resource utilization.
[0021] Advantage 2 of the present invention is that the oxidation liquid generated in the biological oxidation pretreatment process is acidic, with a pH between 1.2 and 1.8. This environment is not conducive to the growth and reproduction of bacteria, which in turn affects the gold extraction production efficiency. Adding electroplating sludge can neutralize the pH of the oxidation liquid, promote the gold extraction production efficiency, and achieve "waste treatment with waste". BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Schematic diagram of the method for pretreatment of electroplating sludge by synergistic bio-oxidation DETAILED DESCRIPTION
[0023] Combination Figure 1 , a clear and complete description of the technical solution in the implementation of this patent. It should be noted that the examples described in the present invention are only used for further explanation and illustration, rather than limiting the scope of its application. Based on the present invention, all other examples obtained by those skilled in the art without creative work are within the scope of protection of the patent of this invention.
[0024] Example 1
[0025] The electroplating sludge in this example is Cu-plated sludge, and its properties are shown in Table 1.
[0026] Table 1 Composition of electroplating sludge with Cu as the plating species used in Example 1
[0027]
[0028] according to Figure 1 Proceed as shown in the steps:
[0029] Step 1: slurry treatment: electroplating sludge and water are mixed in a mass ratio of 1:1 into a slurry machine for stirring at a stirring speed of 300 r / min.
[0030] Step 2: Co-treatment: the electroplating sludge after slurry treatment is added to the biological oxidation liquid at a volume ratio of 1:3 and mixed for reaction for 15 hours.
[0031] Step three: Filtration: The co-processed products are separated into solid and liquid to obtain filtrate and filter residue respectively. The filtrate is fed to the next step of ion exchange, and the filter residue is fed to the subsequent gold extraction operation.
[0032] Step 4: Ion exchange process: The filtrate flows through the exchange column for ion exchange, and the filtrate is always higher than the cation exchange column during the process until the effluent reaches the flow point;
[0033] Step 5: Desorption: The ion exchange column is treated with dilute hydrochloric acid with a mass concentration of 20% to obtain a copper-enriched solution. The copper content is 75% after testing.
[0034] Example 2
[0035] The electroplating sludge used in Example 2 is the same as that in Example 1, and the following steps are performed:
[0036] Step 1: Slurry treatment: electroplating sludge and water are fed into a slurry machine at a mass ratio of 1.2:1 for stirring at a stirring speed of 300 r / min.
[0037] Step 2: Co-treatment: the electroplating sludge after slurry treatment is added to the biological oxidation liquid at a volume ratio of 1:3 and mixed for reaction for 15 hours.
[0038] Step three: Filtration: The co-processed products are separated into solid and liquid to obtain filtrate and filter residue respectively. The filtrate is fed to the next step of ion exchange, and the filter residue is fed to the subsequent gold extraction operation.
[0039] Step 4: Ion exchange process: The filtrate flows through the exchange column for ion exchange, and the filtrate is always higher than the cation exchange column during the process until the effluent reaches the flow point;
[0040] Step 5: Desorption: The ion exchange column is treated with dilute hydrochloric acid with a mass concentration of 20% to obtain a copper-enriched solution. The copper content is 75% after testing.
[0041] Example 3
[0042] The electroplating sludge used in Example 3 is the same as that in Example 1, and the following steps are performed:
[0043] Step 1: Slurry treatment: electroplating sludge and water are fed into a slurry machine at a mass ratio of 1.2:1 for stirring at a stirring speed of 350 r / min.
[0044] Step 2: Co-treatment: the electroplating sludge after slurry treatment is added to the biological oxidation liquid at a volume ratio of 1:3 and mixed for reaction for 15 hours.
[0045] Step three: Filtration: The co-processed products are separated into solid and liquid to obtain filtrate and filter residue respectively. The filtrate is fed to the next step of ion exchange, and the filter residue is fed to the subsequent gold extraction operation.
[0046] Step 4: Ion exchange process: The filtrate flows through the exchange column for ion exchange, and the filtrate is always higher than the cation exchange column during the process until the effluent reaches the flow point;
[0047] Step 5: Desorption: The ion exchange column is treated with dilute hydrochloric acid having a mass concentration of 20% to obtain a copper-enriched solution.
[0048] The copper content in the final enriched solution is 73%.
[0049] Embodiment 4:
[0050] The electroplating sludge used in Example 4 is the same as that in Example 1, and the following steps are performed:
[0051] Step 1: Slurry treatment: electroplating sludge and water are fed into a slurry machine at a mass ratio of 1.2:1 for stirring at a stirring speed of 300 r / min.
[0052] Step 2: Co-treatment: the electroplating sludge after slurry treatment is added to the biological oxidation liquid at a volume ratio of 1:3 and mixed for reaction for 18 hours.
[0053] Step three: Filtration: The co-processed products are separated into solid and liquid to obtain filtrate and filter residue respectively. The filtrate is fed to the next step of ion exchange, and the filter residue is fed to the subsequent gold extraction operation.
[0054] Step 4: Ion exchange process: The filtrate flows through the exchange column for ion exchange, and the filtrate is always higher than the cation exchange column during the process until the effluent reaches the flow point;
[0055] Step 5: Desorption: The ion exchange column is treated with dilute hydrochloric acid with a mass concentration of 20% to obtain a copper-enriched solution. The copper content is 75% after testing.
[0056] Embodiment 5:
[0057] The electroplating sludge in Example 5 is a Zn-plated sludge with a Fe content of 45.97%, a Zn content of 17.33%, and a Sn content of 8.42%. Figure 1 The method shown is carried out:
[0058] Step 1: Slurry treatment: electroplating sludge and water are fed into a slurry machine in a mass ratio of 1:1 for stirring at a stirring speed of 300 r / min.
[0059] Step 2: Co-treatment: the electroplating sludge after slurry treatment is added into the biological oxidation liquid at a volume ratio of 1:3, and the mixed reaction is carried out for 15 hours.
[0060] Step three: Filtration: The co-processed products are separated into solid and liquid to obtain filtrate and filter residue respectively. The filtrate is fed to the next step of ion exchange, and the filter residue is fed to the subsequent gold extraction operation.
[0061] Step 4: Ion exchange process: The filtrate flows through the exchange column for ion exchange, and the filtrate is always higher than the cation exchange column during the process until the effluent reaches the flow point;
[0062] Step 5: Desorption: The ion exchange column was treated with 20% diluted hydrochloric acid to obtain a zinc-enriched solution. The zinc content was 47%.
[0063] Example 6
[0064] The composition of the electroplating sludge in Example 6 is consistent with that in Example 5. Figure 1 The method shown deals with:
[0065] Step 1: Slurry treatment: electroplating sludge and water are fed into a slurry machine at a mass ratio of 1.2:1 for stirring at a stirring speed of 300 r / min.
[0066] Step 2: Co-treatment: the electroplating sludge after slurry treatment is added into the biological oxidation liquid at a volume ratio of 1:3, and the mixed reaction is carried out for 15 hours.
[0067] Step three: Filtration: The co-processed products are separated into solid and liquid to obtain filtrate and filter residue respectively. The filtrate is fed to the next step of ion exchange, and the filter residue is fed to the subsequent gold extraction operation.
[0068] Step 4: Ion exchange process: The filtrate flows through the exchange column for ion exchange, and the filtrate is always higher than the cation exchange column during the process until the effluent reaches the flow point;
[0069] Step 5: Desorption: The ion exchange column was treated with 20% diluted hydrochloric acid to obtain a zinc-enriched solution, and the zinc content was 43%.
[0070] Example 7
[0071] The composition of the electroplating sludge in Example 7 is consistent with that in Example 5. Figure 1 The method shown deals with:
[0072] Step 1: Slurry treatment: electroplating sludge and water are fed into a slurry machine in a mass ratio of 1:1 for stirring at a stirring speed of 350 r / min.
[0073] Step 2: Co-treatment: the electroplating sludge after slurry treatment is added into the biological oxidation liquid at a volume ratio of 1:3, and the mixed reaction is carried out for 15 hours.
[0074] Step three: Filtration: The co-processed products are separated into solid and liquid to obtain filtrate and filter residue respectively. The filtrate is fed to the next step of ion exchange, and the filter residue is fed to the subsequent gold extraction operation.
[0075] Step 4: Ion exchange process: The filtrate flows through the exchange column for ion exchange, and the filtrate is always higher than the cation exchange column during the process until the effluent reaches the flow point;
[0076] Step 5: Desorption: The ion exchange column is treated with dilute hydrochloric acid with a mass concentration of 20% to obtain a zinc-enriched solution. The zinc content is 45% after testing.
[0077] Example 8
[0078] The composition of the electroplating sludge in Example 6 is consistent with that in Example 5. Figure 1 The method shown deals with:
[0079] Step 1: Slurry treatment: electroplating sludge and water are fed into a slurry machine in a mass ratio of 1:1 for stirring at a stirring speed of 300 r / min.
[0080] Step 2: Co-treatment: the electroplating sludge after slurry treatment is added into the biological oxidation liquid at a volume ratio of 1:3, and the mixed reaction is carried out for 18 hours.
[0081] Step three: Filtration: The co-processed products are separated into solid and liquid to obtain filtrate and filter residue respectively. The filtrate is fed to the next step of ion exchange, and the filter residue is fed to the subsequent gold extraction operation.
[0082] Step 4: Ion exchange process: The filtrate flows through the exchange column for ion exchange, and the filtrate is always higher than the cation exchange column during the process until the effluent reaches the flow point;
[0083] Step 5: Desorption: The ion exchange column is treated with dilute hydrochloric acid with a mass concentration of 20% to obtain a zinc-enriched solution. The zinc content is 46% after testing.
Claims
1. A method for pre-treating electroplating sludge by synergistic bio-oxidation. It is characterized in that The following steps are included: Step 1: Slurry treatment: Feed the electroplating sludge and water into a slurry machine for slurry treatment; Step 2, synergistic treatment: feeding the electroplating sludge after pulping treatment into the biological oxidation liquid, mixing and reacting to obtain a synergistic treatment product; Step 3, filtration: performing solid-liquid separation on the co-processed product obtained in step 2 to obtain a filtrate and a filter residue respectively; Step 4, ion exchange process: the filtrate obtained in step 3 is fed into the cation exchange resin from top to bottom, and the valuable metal ions in the filtrate will be adsorbed into the cation exchange resin; Step 5: Desorption: Treat the cation exchange resin with an acid solution to obtain an enriched solution containing copper and zinc ions.
2. The method for pre-treating electroplating sludge by synergistic bio-oxidation according to claim 1, It is characterized in that In the step 1, the ratio of electroplating sludge to water is, by mass ratio, (1-1.8):1, and the stirring speed during slurry treatment is 300-500 r / min.
3. The method for pre-treating electroplating sludge by synergistic bio-oxidation according to claim 1, It is characterized in that In the step 2, the valuable elements are selected from one or more of copper and zinc; the biological oxidation liquid is the biological oxidation liquid produced during the biological oxidation process of the refractory gold ore.
4. The method for pre-treating electroplating sludge by synergistic bio-oxidation according to claim 1, It is characterized in that In the step 2, the ratio of the electroplating sludge after slurry treatment to the biological oxidation liquid is 1:(2-3) by volume; the coordinated treatment temperature is 25-30° C., and the coordinated treatment time is 15-20 hours.
5. The method for pre-treating electroplating sludge by synergistic bio-oxidation according to claim 1, It is characterized in that In the step three, the filtrate contains valuable metal elements in the electroplating sludge, and the filter residue contains the refractory gold ore and suspended matter that is insoluble in acid after being treated with bacteria in the biological oxidation liquid.
6. The method for pre-treating electroplating sludge by synergistic bio-oxidation according to claim 1, It is characterized in that In step 4, during the ion exchange process, the filtrate height needs to be always higher than the cation exchange resin layer. When the effluent concentration of the cation exchange resin reaches the flow point, the filtrate feeding is stopped and the ion exchange is completed.
7. The method for pre-treating electroplating sludge by synergistic bio-oxidation according to claim 1, It is characterized in that In the step 5, the acid solution is selected from inorganic acids, specifically including hydrochloric acid, sulfuric acid, and nitric acid, and the concentration is 5% to 20% by mass.
Citation Information
Patent Citations
Method for recycling heavy metal in electroplating sludge
CN102719657A
No-waste utilization method of heavy metal-contained sludge
CN106987721A
Method for resourceful treatment of electroplating sludge based on nickel recovery
CN111363927A
Sludge and slurry destruction plant and process
WO2002081386A1