High-thermal-conductivity copper-diamond composite material and warm-pressing near-net forming preparation method thereof
Through the temperature-pressure near-net forming process of diamond particles and copper alloy powder covered with metallized coating on the surface, the problems of low production efficiency and high cost of existing copper-diamond composite materials are solved, and high thermal conductivity and bending strength are achieved The preparation of copper-diamond composite materials is suitable for heat dissipation materials of electronic devices.
Patent Information
- Application Number
- CN202410954299.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
The existing copper-diamond composite preparation methods are inefficient and costly, and it is difficult to make large-size special-shaped products. The processing process is complex, which limits its application in heat dissipation of electronic devices.
采用表面包覆金属化涂层的金刚石颗粒与铜合金粉末混合,通过温压近净成形工艺制备高导热铜-金刚石复合材料,利用粗化剂提高金刚石表面粗糙度,增加与铜的结合强度,并通过真空沉积和粘结剂调节烧结收缩率,实现大尺寸异形产品的制备。
Copper-diamond composite materials with high thermal conductivity (500~550W/(m·K) and high bending strength are achieved, which reduces the preparation cost and improves production efficiency. It is suitable for large-scale manufacturing and electronic packaging materials, and reduces processing. The process and improve the preparation efficiency.
Smart Images

Figure CN118880100A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of manufacturing a composite layer, workpiece or product containing metal powder by sintering the metal powder with or without compaction, and specifically relates to a high thermal conductivity copper-diamond composite material and a warm pressing near-net-shape preparation method thereof. Background Art
[0002] As electronic devices develop towards high performance, miniaturization and high integration, traditional heat dissipation materials have gradually become unable to meet the demand, and the heat dissipation problem has become one of the technical bottlenecks restricting the development of the electronic information industry. In order to obtain stable performance, the heat dissipation conditions of electronic devices must be improved, so the research on high-performance heat dissipation materials has become the key to the development of the electronics industry.
[0003] Copper-diamond composites have become a new generation of thermal management materials due to their high thermal conductivity and suitable thermal expansion coefficient. The current method for preparing copper-diamond composites is mainly melt infiltration, in which molten metal copper is infiltrated into the gaps between diamond particle deposits under the action of gas pressure, mechanical extrusion force or capillary force. The shape and size of the product are restricted by the mold, and it is difficult to make large-sized special-shaped products. The hardness of diamond is 10 on the Mohs hardness scale, and the post-processing problem is currently a world-recognized difficulty.
[0004] Patent CN109940156A proposes a method for preparing diamond / copper thermal conductive composite parts by 3D printing near-net shape, which uses 3D printing to prepare a diamond skeleton, and then uses a vacuum pressure infiltration process to fill copper into the skeleton gap to finally prepare a copper-diamond composite material with a certain shape. However, the pressure infiltration process has low production efficiency, high preparation cost, and the product size is still limited by the mold. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a high thermal conductivity copper-diamond composite material and a warm pressing near-net forming preparation method thereof in view of the above-mentioned deficiencies in the prior art. The thermal conductivity of the composite material can meet the heat dissipation requirements of the chip, and the preparation method can prepare copper-diamond composite material products with large-sized special-shaped structures, which solves the problem of high processing difficulty of copper-diamond composite materials in the prior art, can achieve near-net forming and reduce the processing process, and has low preparation cost, high yield rate, and can be manufactured in large quantities.
[0006] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0007] Provided is a high thermal conductivity copper-diamond composite material, which is obtained by dispersing diamond particles with a metallized coating on the surface in a copper alloy, and the volume fraction of diamond in the composite material is 50-70%.
[0008] According to the above scheme, the thermal conductivity of the high thermal conductivity copper-diamond composite material is 500-550W / (m·K), and the thermal expansion coefficient is 6.0×10 -6 ~7.0×10 -6 / ℃, flexural strength is 350~380MPa, and density is 98~98.5%.
[0009] According to the above scheme, the surface coating thickness of the diamond particles coated with the metallized coating is 300-600nm.
[0010] The present invention also provides a method for preparing the above-mentioned high thermal conductivity copper-diamond composite material by warm pressing near-net forming, and the specific preparation steps are as follows:
[0011] Step 1, roughening the surface of diamond particles: mixing and stirring the diamond particles and the roughening agent, and then laying them in an alumina ceramic crucible, and then placing the alumina ceramic crucible in a muffle furnace for heat treatment, and the obtained product is taken out and cleaned after natural cooling to obtain diamond particles with roughened surfaces;
[0012] Step 2: Surface metallization of diamond particles: The roughened diamond particles obtained in step 1 are mixed with pre-plated metal mixed powder and mixed salt and then placed in a vacuum tube furnace for vacuum deposition reaction to obtain diamond particles with a metallized coating on the surface;
[0013] Step 3, preparing copper diamond feed particles: mixing the diamond particles coated with the metallized coating obtained in step 2 with copper alloy powder and a binder, and adding them into a vacuum internal mixer for internal mixing. After the internal mixing is completed, the copper diamond feed particles with a particle size of 0.5 to 1 mm are formed by a granulator;
[0014] Step 4: Prepare a high thermal conductivity copper-diamond composite material by isothermal near-net forming: Fill the copper-diamond feed particles obtained in step 3 into a forming mold for warm pressing, and obtain a copper-diamond blank after demolding. The copper-diamond blank is then degreased and sintered to obtain a high thermal conductivity copper-diamond composite material.
[0015] According to the above scheme, the particle size of the diamond particles in step 1 is 100 to 500 μm, preferably 100 to 300 μm.
[0016] According to the above scheme, the components and mass percentage of the coarsening agent in step one are: 30-50% Fe2O3 powder, 50-70% MnO2 powder, and the particle size of Fe2O3 powder and MnO2 powder is 1-20 μm, preferably 5-10 μm.
[0017] According to the above scheme, the mass ratio of diamond particles to roughening agent in step 1 is 1:3-5.
[0018] According to the above scheme, the heat treatment process conditions in step 1 are: heating to 600-800°C at a heating rate of 5-20°C / min at room temperature, and keeping warm for 30-60 minutes.
[0019] According to the above scheme, the pre-plated metal mixed powder in step 2 is a mixture of metal powder and its oxide powder, wherein the metal powder is selected from one of Ti powder, Cr powder, Mo powder and W powder, and the corresponding oxide powders are TiO2 powder, Cr2O3 powder, MoO2 powder and WO3 powder respectively. The particle size of the metal powder is 1 to 10 μm, preferably 3 to 5 μm, the particle size of the oxide powder is 1 to 10 μm, preferably 3 to 5 μm, and the mass percentage of the metal powder in the pre-plated metal mixed powder is 20 to 50%.
[0020] According to the above scheme, the particle size of the mixed salt in step 2 is 300-400 mesh, and the components and mass percentages are: 30-40% NH4Cl powder, 30-40% NaCl powder, and 20-40% KCl powder.
[0021] According to the above scheme, the surface roughened diamond particles described in step 2 are mixed with pre-plated metal mixed powder and mixed salt, and the mass percentage of each component is: surface roughened diamond particles 30-60%, pre-plated metal mixed powder 20-50%, and mixed salt 5-20%.
[0022] Preferably, the surface roughened diamond particles in step 2 are mixed with pre-plated metal mixed powder and mixed salt, and the mass percentage of each component is: surface roughened diamond particles 50-60%, pre-plated metal mixed powder 30-40%, and mixed salt 10-20%.
[0023] According to the above scheme, the process conditions of the vacuum deposition reaction in step 2 are: vacuum degree <1Pa, heating to 800-1200°C at a heating rate of 5-10°C / min at room temperature, and deposition for 30-60 minutes.
[0024] According to the above scheme, the copper alloy powder in step three has a particle size of 3-10 μm, and its composition and mass percentage are: B 0.50-1.20%, Ti 0.15-0.55%, Ag 4.50-8.00%, Ni 0.50-1.50%, Cr 0.60-1.20%, and the balance is Cu.
[0025] According to the above scheme, the binder components and mass percentages in step three are: polyethylene glycol (molecular weight 1000-2000), 20-40% (preferably 30-35%), polyoxymethylene (molecular weight 30,000-40,000) 10-30% (preferably 20-25%), polyethylene (molecular weight 200,000-250,000) 10-20% (preferably 15-20%), ethylene-vinyl acetate copolymer (number average molecular weight 150-350), 20-30% (preferably 25-30%), and 80# microcrystalline wax 1-10% (preferably 5-10%).
[0026] According to the above scheme, in step three, the diamond particles coated with metallized coating are mixed with copper alloy powder and binder, and the mass percentage of each component is as follows: 35-50% of diamond particles coated with metallized coating, 45-60% of copper alloy powder, and 5-10% of binder.
[0027] According to the above scheme, the mixing process conditions in step three are: vacuum degree 1-20 Pa, mixing temperature 140-180° C., and mixing time 2-4 h.
[0028] According to the above scheme, the warm pressing forming process conditions in step four are: temperature of 140-180°C, pressure of 300-600MPa, and holding time of 10-30s.
[0029] According to the above scheme, the degreasing method in step 4 is: solvent degreasing and high temperature degreasing are used. The solvent used for solvent degreasing is: one or a mixture of n-heptane, 1,2,3-tribromopropane, acetone, and toluene. The solvent degreasing temperature is 35-50°C, and the degreasing time is 4-6h.
[0030] The high-temperature degreasing process conditions are: heating to 450-500°C at a heating rate of 5-10°C / min at room temperature, keeping warm for 1-2 hours, then heating to 800-900°C at a heating rate of 3-5°C / min, introducing hydrogen (purity >99.95vol%) after reaching the temperature, and keeping warm for 0.5-1h.
[0031] According to the above scheme, the sintering process conditions in step 4 are: vacuum degree 10 -5 ~10 -3 Pa, heat up to 650-700°C at a heating rate of 1-3°C / min, keep warm for 30-60min, then heat up to 950-1050°C at a heating rate of 0.5-1°C / min, keep warm for 60-180min, cool down to 600-700°C and keep warm for 120-240min.
[0032] The present invention also includes the application of the above-mentioned high thermal conductivity copper-diamond composite material in electronic packaging materials.
[0033] In diamond crystals, carbon atoms are interconnected in a tetrahedral bonding manner and the CC bond is very strong, indicating that diamond has a certain stability. During the preparation of copper-diamond composite materials, the poor wettability of diamond leads to weak bonding between copper and diamond. The present invention uses a relatively cheap metal oxide as a roughening agent to perform surface etching on a diamond single crystal at high temperature. The increase in the roughness of the diamond surface after etching can effectively improve the holding force of metal copper on diamond. At the same time, the specific surface area of the diamond after the roughening treatment of the present invention increases, which increases the contact area and bonding strength between diamond and copper, and improves the thermal conductivity and mechanical properties of the copper-diamond composite material.
[0034] Diamond surface metallization adopts vacuum reaction deposition process. Metal oxide has a certain saturated vapor pressure in a vacuum environment at a certain temperature. Metal oxide evaporates and adheres to the diamond surface. At the same time, the carbon atoms on the diamond surface reduce the metal oxide to metal atoms. Finally, the metal atoms and carbon atoms form metal carbides wrapped on the diamond surface. A certain amount of mixed salt is added during vacuum deposition to isolate excess oxygen. At the same time, the salt vapor carries the metal oxide vapor to volatilize at high temperature, making the coating more uniform.
[0035] The warm pressing near-net forming technology is used to control the sintering shrinkage of copper diamond by adjusting the amount of binder added, and finally the product size is artificially controlled while sintering densely. Since the polymer binder is added to the feed, the solvent degreasing and high-temperature degreasing are used to complete the degreasing process in coordination. The binder residue after degreasing in this process is less than 0.05%.
[0036] The copper-diamond composite material prepared by the present invention adopts a vacuum activated sintering process, and the copper alloy powder contains a certain amount of activated elements such as B, Ti, Ni, Cr, Ag, etc. The added Ag and B elements can reduce the melting point of copper, change the fluidity of copper in a molten state, and metal copper fills the gaps between diamond particles and wraps the diamond particles under the action of capillary tension. Ti, Cr, and Ni elements react with the metal layer on the surface of diamond under the action of concentration gradient to form a solid solution, and at the same time, the interface between diamond and copper forms a metallurgical bond. The addition of such elements enhances the interfacial bonding strength between diamond and copper matrix and improves thermal conductivity.
[0037] The beneficial effects of the present invention are as follows: 1. The copper-diamond composite material provided by the present invention has good application prospects in the field of electronic packaging materials due to its good thermal conductivity (>500W / mK). 2. The present invention adopts a warm pressing near-net forming process, the process equipment is simple, can be operated continuously, has high production efficiency, and has a high degree of automation. The copper-diamond composite material can be manufactured in large quantities and at low cost. The circular size tolerance is ±0.1mm, which is suitable for preparing large-sized and special-shaped copper-diamond composite materials, which is convenient for the processing and preparation of subsequent products, effectively reducing the processing steps while improving the preparation efficiency and reducing the preparation cost. In addition, the copper-diamond feed particles can be recycled, which greatly reduces the manufacturing cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a SEM comparison image of the diamond particles used in Example 1 and the diamond particles with roughened surfaces obtained in step 1;
[0039] Figure 2 This is a cross-sectional SEM image of the diamond particles coated with a coating on the surface obtained in step 2 of Example 1;
[0040] Figure 3 This is an EDS spectrum of the surface coating of the diamond particles coated with a coating obtained in step 2 of Example 1;
[0041] Figure 4 This is a physical picture of the isothermal near-net-shape high thermal conductivity copper-diamond composite material of Example 1. DETAILED DESCRIPTION
[0042] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings.
[0043] Example 1
[0044] A high thermal conductivity copper-diamond composite material, the specific preparation method is as follows:
[0045] Step 1, roughening the surface of diamond particles: diamond particles (particle size 200 μm) and a roughening agent are mixed and stirred in a mass ratio of 1:4 and laid in an alumina ceramic crucible, wherein the composition and ratio of the roughening agent are: 40 wt.% of Fe2O3 powder and 60 wt.% of MnO2 powder, and the powder particle size is 5-8 μm. Then, the alumina ceramic crucible is placed in a muffle furnace, and the temperature is increased to 800°C at a heating rate of 10°C / min at room temperature for heat treatment for 60 minutes. After natural cooling, the obtained product is cleaned to obtain diamond particles with roughened surface;
[0046] Step 2, surface metallization of diamond particles: the surface roughened diamond particles obtained in step 1 are mixed with pre-plated metal mixed powder and mixed salt, and then placed in a vacuum tube furnace for vacuum deposition. The raw materials and proportions are as follows: 50wt.% of surface roughened diamond particles, 40wt.% of pre-plated metal mixed powder, and 10wt.% of mixed salt, wherein the pre-plated metal mixed powder is obtained by mixing 45wt.% of metal Cr powder and 55wt.% of Cr2O3 powder, and the powder particle size is 3-5μm; the mixed salt is obtained by mixing 15wt.% of NH4Cl powder, 38wt.% of NaCl powder and 47wt.% of KCl powder, and the particle size is 300-400 meshes. The vacuum reaction deposition process conditions are: vacuum degree 0.15Pa, heating to 900℃ at a heating rate of 8℃ / min at room temperature for deposition, and deposition time 60min, to obtain diamond particles with Cr3C2-Cr coating on the surface, and the coating thickness is 400-600nm;
[0047] Step 3, preparing copper diamond feed particles: 55wt.% copper alloy powder, 37wt.% diamond particles with a coating prepared in step 2, and 8wt.% binder are mixed and added into a vacuum mixer for internal mixing. After internal mixing, copper diamond feed particles with a particle size of 0.8mm are formed by a granulator. The copper alloy powder used is vacuum atomized powder with a particle size of 3-5μm and the composition is: B 0.88wt.%, Ti 0.45wt.%, Ag 6.74wt.%, Ni 1.23wt.%, Cr 0.93wt.%, the balance is Cu; the binder components and proportions are: PEG2000 polyethylene glycol (purchased from Shanghai Huijun Chemical Co., Ltd.) 32wt.%, polyoxymethylene (purchased from Ningbo Zhengzhang Chemical Co., Ltd., POM-25) 23wt.%, polyethylene (Yanshan Petrochemical injection molding grade LD400) 15wt.%, ethylene-vinyl acetate copolymer (Japan Mitsui Chemicals, V961RC) 25wt.%, 80# microcrystalline wax (purchased from Yangzhou Roland New Materials Co., Ltd.) 5wt.%, the vacuum degree of the mixer is 5Pa, the mixing temperature is 170℃, and the mixing time is 3h;
[0048] Step 4: Preparation of high thermal conductivity copper-diamond composite material by isothermal near-net forming: The copper-diamond feed particles obtained in step 3 are filled into a forming mold for warm pressing, with a mold temperature of 145° C., a pressure of 450 MPa, and a holding time of 20 s. After demolding, a copper-diamond blank with a diameter of 22 mm and a thickness of 3 mm is obtained;
[0049] Step 5, degreasing: The copper diamond blank is immersed in n-heptane at 35°C for 4 hours to remove most of the binder, and then placed in a degreasing furnace for high-temperature degreasing. The process conditions are: heating to 480°C at a rate of 5°C / min at room temperature for 2 hours, and then heating to 900°C at a rate of 3°C / min. After reaching the temperature, hydrogen (purity 99.999 vol%) is introduced, and the temperature is kept for 1 hour. After cooling, the copper diamond degreased blank is obtained.
[0050] Step 6: Sintering: Place the copper diamond degreased embryo into a vacuum sintering furnace for activation sintering. The vacuum activation sintering process is: vacuum degree 3.5×10 -4 Pa, heated to 650°C at a rate of 3°C / min at room temperature, kept warm for 30min, then heated to 1020°C at a rate of 1°C / min, kept warm for 120min, cooled to 880°C for solution treatment for 240min, and sintered to obtain a high thermal conductivity copper-diamond composite material with a diameter of 20mm and a height of 2.7mm.
[0051] Figure 1 This is a SEM comparison of the diamond particles used in this example (left) and the surface-roughened diamond particles obtained in step 1 (right). It can be seen that the diamond surface is overall rough and uneven after the roughening treatment, and the specific surface area is significantly increased.
[0052] Figure 2 This is a cross-sectional SEM image of the diamond particles coated with a coating obtained in step 2 of this embodiment. Figure 3 This is the EDS energy spectrum of the surface coating of diamond particles. It can be seen that the surface of the diamond particles is covered with a uniform "Cr3C2-Cr" coating with a coating thickness of 400 to 500 nm.
[0053] Figure 4 This is a physical picture of the isothermal near-net-formed high thermal conductivity diamond copper composite material of this embodiment. The high thermal conductivity diamond copper composite material is a disc with a diameter of 20 mm. Diamonds are evenly distributed in the composite material and account for a high proportion. According to calculation, the volume fraction of diamonds in the composite material is 63%.
[0054] After testing, the copper-diamond composite material obtained in this embodiment has a thermal conductivity of 526 W / mK, a thermal expansion coefficient of 6.8 ppm / °C, a flexural strength of 389 MPa, a density of 98.2%, a sample deformation (thickness direction) after sintering of 1.4%, and a circular size tolerance of ±0.08 mm.
[0055] Example 2
[0056] A high thermal conductivity copper-diamond composite material, the preparation method of which by warm pressing near-net forming is as follows:
[0057] Step 1, roughening the surface of diamond particles: diamond particles (particle size 300 μm) and a roughening agent are mixed and stirred in a mass ratio of 1:4 and laid in an alumina ceramic crucible, wherein the composition and ratio of the roughening agent are: 50 wt.% of Fe2O3 powder and 50 wt.% of MnO2 powder, and the powder particle size is 5-8 μm. Then, the alumina ceramic crucible is placed in a muffle furnace, heated to 780°C at a heating rate of 10°C / min at room temperature for heat treatment for 50 minutes, and after natural cooling, the obtained product is cleaned to obtain diamond particles with roughened surface;
[0058] Step 2, surface metallization of diamond particles: the surface roughened diamond particles obtained in step 1 are mixed with pre-plated metal mixed powder and mixed salt, and then placed in a vacuum tube furnace for vacuum deposition. The raw materials and proportions are as follows: 50wt.% of surface roughened diamond particles, 40wt.% of pre-plated metal mixed powder, and 10wt.% of mixed salt, wherein the pre-plated metal mixed powder is obtained by mixing 40wt.% of metal W powder and 60wt.% of WO3 powder, and the powder particle size is 3-5μm; the mixed salt is obtained by mixing 10wt.% NH4Cl powder, 40wt.% NaCl powder and 50wt.% KCl powder, and the particle size is 300-400 meshes. The vacuum reaction deposition process conditions are: vacuum degree 0.15Pa, heating at a heating rate of 8℃ / min at room temperature to 1150℃ for deposition, and the deposition time is 60min, to obtain diamond particles with a "WC-W" coating on the surface, and the coating thickness is 300-400nm;
[0059] Step 3, preparing copper diamond feed particles: 55wt.% copper alloy powder, 37wt.% of the diamond particles with metallized coating prepared above, and 8wt.% of binder are mixed and added into a vacuum mixer for internal mixing. After internal mixing, copper diamond feed particles with a particle size of 1mm are formed by a granulator. The copper alloy powder used is vacuum atomized powder with a particle size of 3-5μm and the composition is: B 0.88wt.%, Ti 0.45wt.%, Ag 6.74wt.%, Ni 1.23wt.%, Cr0.93wt.%, the balance is Cu; the binder composition and proportion are: polyethylene glycol (PEG2000) 32wt.%, polyoxymethylene (POM-25) 23wt.%, polyethylene 15wt.%, ethylene-vinyl acetate copolymer 25wt.%, 80# microcrystalline wax 5wt.%; the vacuum degree of the internal mixer is 5Pa, the internal mixing temperature is 170℃, and the internal mixing time is 3h;
[0060] Step 4: Preparation of high thermal conductivity copper-diamond composite material by isothermal near-net forming: The copper-diamond feed particles obtained in step 3 are filled into an isothermal forming mold for warm pressing, with a mold temperature of 150°C, a pressure of 500 MPa, and a holding time of 30 seconds. After demolding, a copper-diamond blank with a diameter of 22 mm and a thickness of 3 mm is obtained.
[0061] Step 5, degreasing: The copper diamond blank is immersed in n-heptane and kept at 35°C for 4 hours to remove most of the binder, and then placed in a degreasing furnace for high-temperature degreasing. The process conditions are: heating to 480°C at a rate of 5°C / min at room temperature for 2 hours, and then heating to 900°C at a rate of 3°C / min. After reaching the temperature, hydrogen is introduced and kept for 1 hour. After cooling, the copper diamond degreased blank is obtained.
[0062] Step 6: Sintering: Place the copper diamond degreased embryo into a vacuum sintering furnace for activation sintering. The vacuum activation sintering process is: vacuum degree 3.5×10 -4 Pa, heated to 650°C at a rate of 3°C / min at room temperature, kept warm for 30 minutes, then heated to 1030°C at a rate of 1°C / min, kept warm for 120 minutes, cooled to 900°C for solution treatment for 240 minutes, and sintered to obtain a high thermal conductivity copper-diamond composite material with a diameter of 20 mm and a height of 2.7 mm.
[0063] After testing, the copper-diamond composite material obtained in this embodiment has a thermal conductivity of 568 W / mK, a thermal expansion coefficient of 6.4 ppm / °C, a flexural strength of 352 MPa, a density of 98.3%, a circular size tolerance of ±0.09 mm, and a sample deformation (thickness direction) of 1.2% after sintering.
[0064] Comparative Examples 1-4
[0065] The diamond surface roughening process in Example 1 was changed, and the other conditions were the same as those in Example 1. The copper-diamond composite material prepared was subjected to comparative tests. The comparative results of Example 1 and Comparative Examples 1-4 are shown in Table 1.
[0066] Table 1
[0067] sample Roughening temperature Roughening time Product Performance Example 1 800℃ 60min The roughening effect is good, the thermal conductivity of the sample is 526W / mK, and the bending strength is 389MPa Comparative Example 1 500℃ 60min The roughening effect is not obvious, the thermal conductivity of the sample is 420W / mK, and the flexural strength is 262MPa Comparative Example 2 1000℃ 60min The temperature is too high and cracks appear in the diamond. The thermal conductivity of the sample is 326W / mK and the bending strength is 163MPa Comparative Example 3 800℃ 10min The roughening effect is not obvious, the thermal conductivity of the sample is 463W / mK, and the bending strength is 322MPa Comparative Example 4 800℃ 120min Diamond cracks appear after a long time. The thermal conductivity of the sample is 389W / mK and the bending strength is 186MPa
[0068] Comparative Examples 5-8
[0069] The vacuum deposition process in Example 1 was changed, and the other conditions were the same as those in Example 1. The diamond particles with the surface coated with the metallized coating were prepared for comparative test. The comparative results of Example 1 and Comparative Examples 5-8 are shown in Table 2.
[0070] Table 2
[0071]
[0072]
[0073] Comparative Examples 9-10
[0074] The raw material ratio of the copper diamond feed particles in Example 1 was changed, and the other conditions were the same as those in Example 1. A copper-diamond composite material was prepared for comparative test. The comparative results of Example 1 and Comparative Examples 9-10 are shown in Table 3.
[0075] Table 3
[0076]
[0077] Comparative Examples 11-15
[0078] The warm pressing parameters in Example 1 were changed, and the other conditions were the same as those in Example 1, to prepare copper-diamond composite materials for comparative tests. The comparison results of the samples after demolding of Example 1 and Comparative Examples 11-15 are shown in Table 4.
[0079] Table 4
[0080] sample Mold temperature pressure Holding time Sample performance after demoulding Example 1 145℃ 450MPa 20s After demoulding, the sample has no defects such as cracks and pores Comparative Example 11 100℃ 450MPa 20s The sample has cracks after demoulding Comparative Example 12 200℃ 450MPa 20s The binder overflowed from the mold during the pressing process and the sample could not be demolded Comparative Example 13 145℃ 200MPa 20s The sample has pore defects after demoulding Comparative Example 14 145℃ 800MPa 20s The mold is stuck and the sample cannot be demoulded Comparative Example 15 145℃ 45MPa 5s The sample is filled unevenly and has pores in the middle
[0081] Comparative Examples 16-19
[0082] The activation sintering process in Example 1 was changed, and the other conditions were the same as those in Example 1 to prepare copper-diamond composite materials for comparative tests. The comparative results of the samples after demolding of Example 1 and Comparative Examples 16-19 are shown in Table 5.
[0083] Table 5
[0084]
[0085]
[0086] It can be seen from Tables 1-5 above that the diamond surface roughening process, diamond surface vacuum deposition process, copper diamond feed particle raw material ratio, warm pressing forming process and activated sintering process all have an impact on product performance. Inappropriate process conditions will lead to product defects and poor performance.
Claims
1. A high thermal conductivity copper-diamond composite material, characterized in that: The high thermal conductivity copper-diamond composite material is obtained by dispersing diamond particles with metallized coatings on the surface in a copper alloy, and the volume fraction of diamond in the composite material is 50-70%.
2. The high thermal conductivity copper-diamond composite material according to claim 1, characterized in that: The high thermal conductivity copper-diamond composite material has a thermal conductivity of 500-550 W / (m·K) and a thermal expansion coefficient of 6.0×10 -6 ~7.0×10 -6 / ℃, flexural strength is 350~380MPa, and density is 98~98.5%.
3. The high thermal conductivity copper-diamond composite material according to claim 1, characterized in that: The thickness of the surface coating of the diamond particles coated with the metallized coating is 300-600nm.
4. A method for preparing a high thermal conductivity copper-diamond composite material by warm pressing and near-net forming according to any one of claims 1 to 3, characterized in that: The specific preparation steps are as follows: Step 1, roughening the surface of diamond particles: mixing and stirring the diamond particles and the roughening agent, and then laying them in an alumina ceramic crucible, and then placing the alumina ceramic crucible in a muffle furnace for heat treatment, and the obtained product is taken out and cleaned after natural cooling to obtain diamond particles with roughened surfaces; Step 2: Surface metallization of diamond particles: The roughened diamond particles obtained in step 1 are mixed with pre-plated metal mixed powder and mixed salt and then placed in a vacuum tube furnace for vacuum deposition reaction to obtain diamond particles with a metallized coating on the surface; Step 3, preparing copper diamond feed particles: mixing the diamond particles coated with the metallized coating obtained in step 2 with copper alloy powder and a binder, and adding them into a vacuum internal mixer for internal mixing. After the internal mixing is completed, the copper diamond feed particles with a particle size of 0.5 to 1 mm are formed by a granulator; Step 4: Prepare a high thermal conductivity copper-diamond composite material by isothermal near-net forming: Fill the copper-diamond feed particles obtained in step 3 into a forming mold for warm pressing, and obtain a copper-diamond blank after demolding. The copper-diamond blank is then degreased and sintered to obtain a high thermal conductivity copper-diamond composite material.
5. The method for preparing a high thermal conductivity copper-diamond composite material by warm pressing and near-net forming according to claim 4, characterized in that: The particle size of the diamond particles in step 1 is 100-500 μm; the components and mass percentage of the coarsening agent in step 1 are: 30-50% Fe2O3 powder, 50-70% MnO2 powder, and the particle size of Fe2O3 powder and MnO2 powder is 1-20 μm; the mass ratio of the diamond particles to the coarsening agent in step 1 is 1:3-5; the heat treatment process conditions in step 1 are: heating to 600-800°C at a heating rate of 5-20°C / min at room temperature, and keeping warm for 30-60 minutes.
6. The method for preparing a high thermal conductivity copper-diamond composite material by warm pressing and near-net forming according to claim 4, characterized in that: The pre-plated metal mixed powder in step 2 is a mixture of metal powder and its oxide powder, wherein the metal powder is selected from one of Ti powder, Cr powder, Mo powder and W powder, and the corresponding oxide powders are TiO2 powder, Cr2O3 powder, MoO2 powder and WO3 powder, respectively. The particle size of the metal powder is 1-10 μm, the particle size of the oxide powder is 1-10 μm, and the mass percentage of the metal powder in the pre-plated metal mixed powder is 20-50%; the particle size of the mixed salt in step 2 is 300-400 mesh, and the components and mass percentage are: NH4Cl The invention discloses a method for preparing the surface roughened diamond particles, wherein the surface roughened diamond particles are 30-40% of the surface roughened diamond particles, the pre-plated metal mixed powder is 30-40% of the surface roughened diamond particles, the pre-plated metal mixed powder is 20-50% of the surface roughened metal mixed powder, and the mixed salt is 5-20% of the surface roughened diamond particles. The process conditions for the vacuum deposition reaction in the step 2 are as follows: the vacuum degree is less than 1 Pa, the temperature is increased to 800-1200° C. at a heating rate of 5-10° C. / min at room temperature, and the deposition is carried out for 30-60 minutes.
7. The method for preparing a high thermal conductivity copper-diamond composite material by warm pressing and near-net forming according to claim 4, characterized in that: Step 3: The copper alloy powder has a particle size of 3-10 μm, and its composition and mass percentage are: B 0.50-1.20%, Ti 0.15-0.55%, Ag 4.50-8.00%, Ni 0.50-1.50%, Cr 0.60-1.20%, the balance is Cu; the binder components and mass percentages in step 3 are: polyethylene glycol 20-40%, polyoxymethylene 10-30%, polyethylene 10-20%, ethylene-vinyl acetate copolymer 20-30%, 80# microcrystalline wax 1-10%; in step 3, the diamond particles coated with a metallized coating on the surface are mixed with copper alloy powder and a binder, and the components and mass percentages are as follows: 35-50% of diamond particles coated with a metallized coating on the surface, 45-60% of copper alloy powder, and 5-10% of a binder; the mixing process conditions in step 3 are: vacuum degree 1-20Pa, banburying temperature 140-180°C, and banburying time 2-4h.
8. The method for preparing a high thermal conductivity copper-diamond composite material by warm pressing and near-net forming according to claim 4, characterized in that: The process conditions of warm pressing in step 4 are as follows: temperature of 140-180°C, pressure of 300-600MPa, and holding time of 10-30s; the degreasing method in step 4 is as follows: solvent degreasing and high temperature degreasing are used for degreasing.
9. The method for preparing a high thermal conductivity copper-diamond composite material by warm pressing and near-net forming according to claim 4, characterized in that: Step 4 Sintering process conditions: vacuum degree 10 -5 ~10 -3 Pa, heat up to 650-700°C at a heating rate of 1-3°C / min, keep warm for 30-60min, then heat up to 950-1050°C at a heating rate of 0.5-1°C / min, keep warm for 60-180min, cool down to 600-700°C and keep warm for 120-240min.
10. Use of the high thermal conductivity copper-diamond composite material according to any one of claims 1 to 3 in electronic packaging materials.
Citation Information
Patent Citations
Near-net forming method for preparing diamond / copper heat-conducting composite material part through 3D printing
CN109940156A
Cited By
Directional heat conduction copper-based diamond composite material and preparation method thereof
CN122303791A
A directional thermally conductive copper-based diamond composite material and its preparation method
CN122303791B