Heat-treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy and preparation method thereof
By adjusting the element ratio and process parameters in aluminum-silicon alloys, high strength and high plasticity under heat-free treatment conditions are achieved, and the problem of improving strength and plasticity of aluminum-silicon alloys under heat-free treatment is solved. It is suitable for complex-shaped castings Production.
Patent Information
- Application Number
- CN202410955243.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to improve the strength and plasticity of aluminum-silicon alloys under heat-free conditions, and the limitations of heat treatment equipment and stress release lead to deformation and quality problems of castings.
Using a specific composition of subeutectic aluminum-silicon alloy, the sub-radar solidification process is performed by controlling the proportion and process parameters of elements such as Si, Mg, Mn, Sr, Ce, Zr, Ti, etc., to regulate the morphology and primary α of eutectic silicon. -Refinement of Al grains to avoid stress release and pore formation.
The alloy is achieved with high strength and high plasticity, with yield strength ≥134MPa, tensile strength ≥271MPa, and elongation ≥12.5%. It is suitable for large-scale production of large and complex-shaped castings.
Smart Images

Figure BDA0004948554600000061
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of metal material processing, and in particular relates to a heat treatment-free high-strength and toughness cast hypoeutectic aluminum-silicon alloy and a preparation method thereof. Background Art
[0002] With the continuous development of economy and society, the fields of aerospace, weaponry, automobiles, etc. have also entered the development stage with high quality requirements, and castings are gradually developing towards integration, large size, thin wall, and complex structure. Heat treatment is the most commonly used working method to improve the mechanical properties of alloy components. Due to the limitation of the volume or shape of heat treatment equipment, large-scale, thin-walled aluminum alloy die-castings formed in one piece are not suitable for heat treatment or irregular-shaped aluminum alloys are difficult to heat treat. In addition, due to stress release, self-quenching and other phenomena during the heat treatment process, castings have quality problems such as deformation and blistering. If the existing technology does not use heat treatment technology to obtain heat-treatment-free aluminum alloy die-casting structural parts, it is difficult to achieve the improvement of the mechanical properties of the alloy, mainly referring to the difficulty in achieving simultaneous improvement of strength and plasticity.
[0003] Therefore, how to reduce alloy costs, simplify the preparation process, avoid the occurrence of quality problems such as stress release, self-quenching, casting deformation, and blistering, and simultaneously improve the strength and plasticity of heat-treatment-free aluminum-silicon alloys is a technical problem that needs to be solved urgently. Summary of the Invention
[0004] In order to solve the above technical problems, the present invention provides a heat-treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy, which is composed of the following components, calculated by mass percentage: Si: 6.0-10.0wt.%, Mg: 0.10-0.50wt.%, Mn: 0.10-0.50wt.%, Sr: 0.02-0.09wt.%, Ce: 0.02-0.06wt.%, Zr: 0.08-0.14wt.%, Ti: 0.08-0.14wt.%, inevitable impurity content ≤0.2wt.%, and the balance is Al; the preparation method of the alloy comprises the following steps:
[0005] Step 1: Melt pure aluminum ingot, Al-20Si master alloy, and Al-10Mn master alloy at 760-810° C. and let stand for 20-70 minutes; then add pure Mg, Al-10Zr master alloy, and Al-10Ti master alloy in sequence at 700-740° C., stir evenly, and let stand for 10-50 minutes to obtain aluminum-silicon alloy melt 1;
[0006] Step 2: Add Al-10Ce master alloy and Al-10Sr master alloy to the aluminum-silicon alloy melt 1 obtained in step 1 at 700-740° C., stir evenly, and let stand for 5-30 minutes to obtain aluminum-silicon alloy melt 2;
[0007] Step 3: heating the aluminum-silicon alloy melt 2 obtained in step 2 to 730-770° C., wrapping the refining agents C2Cl6 and KF with aluminum foil, pressing the refining agents C2Cl6 and KF to the bottom of the melt 2 with a pressure cover, stirring for 3-10 minutes, and standing for 5-20 minutes to obtain an aluminum-silicon alloy melt 3;
[0008] Step 4: Cool the aluminum-silicon alloy melt 3 obtained in step 3 to 710-740° C., introduce high-purity argon gas, perform degassing and impurity removal refining treatment, and keep the temperature for 5-15 minutes to obtain an aluminum-silicon alloy melt 4;
[0009] Step 5: The aluminum-silicon alloy melt 4 obtained in step 4 is poured into a water-cooled copper mold for sub-rapid solidification at 690-720° C. to obtain a heat-treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy. The sub-rapid solidification is as follows: the sub-rapid solidification rate is 80-450° C. / s;
[0010] The mass ratio of C2Cl6 and KF in step 3 is 2:1 to 4:1; the mass ratio of C2Cl6 and KF in the aluminum-silicon alloy melt 3 is 0.2-1%.
[0011] Furthermore, in terms of mass percentage, the material is composed of the following components: Si: 7.0-9.0wt.%, Mg: 0.20-0.40wt.%, Mn: 0.20-0.40wt.%, Sr: 0.05-0.07wt.%, Ce: 0.03-0.05wt.%, Zr: 0.09-0.12wt.%, Ti: 0.09-0.12wt.%, and the balance is Al.
[0012] Furthermore, the pure aluminum ingot, Al-20Si master alloy, and Al-10Mn master alloy described in step 1 are melted at 780-800°C and allowed to stand for 30-60 minutes; pure Mg, Al-10Zr master alloy, and Al-10Ti master alloy are added in sequence at 720-730°C, stirred evenly, and allowed to stand for 20-30 minutes to obtain an aluminum-silicon alloy melt 1.
[0013] Furthermore, the aluminum-silicon alloy melt 1 described in step 2 is added with Al-10Ce master alloy and Al-10Sr master alloy at 720-730° C. and allowed to stand for 10-25 minutes to obtain the aluminum-silicon alloy melt 2.
[0014] Furthermore, step 3 describes heating the aluminum-silicon alloy melt 2 to 740-760°C, wrapping the refining agents C2Cl6 and KF with aluminum foil, pressing the refining agents C2Cl6 and KF to the bottom of the melt 2 with a pressure cover, stirring for 4-7 minutes, and standing for 6-15 minutes.
[0015] Furthermore, step 4 is to cool the aluminum-silicon alloy melt 3 to 720-730° C., introduce high-purity argon gas, perform degassing and impurity removal refining treatment, and keep the temperature for 6-10 minutes.
[0016] Furthermore, the aluminum-silicon alloy melt 4 described in step 5 is poured into a water-cooled copper mold at 700-710° C. for sub-rapid solidification to obtain a high-strength and plastic casting hypoeutectic aluminum-silicon alloy.
[0017] Furthermore, the sub-rapid solidification rate in step 5 is 100-300°C / s.
[0018] Compared with the prior art, the present invention has the following excellent effects:
[0019] Prior art reports indicate that the mechanical properties of Al-Si-Mn-Mg alloys are relatively poor among aluminum alloy systems. This is primarily due to the fact that Si exists in the hypoeutectic aluminum-silicon alloy as a slender, needle-shaped, brittle, hard phase, eutectic silicon, which is relatively coarse. Therefore, as the second phase with the highest content in the hypoeutectic aluminum-silicon alloy, the content and slender, needle-like morphology of eutectic silicon inevitably affect the alloy's performance. Therefore, it is highly effective to regulate the alloy's structure and improve its performance. However, the traditional modification process, which uses Na for modification, produces strong aspiration, increasing the probability and number of pores in the casting, which is detrimental to the casting quality, leading to unstable mechanical properties and adversely affecting the alloy's strength and plasticity. Furthermore, the addition of Sb to the alloy refines the eutectic silicon but does not change its morphology, thus failing to effectively improve the alloy's mechanical properties.
[0020] Compared with the existing technology, the present invention has the following advantages through the synergistic regulation of the interaction between alloy components, proportions, processes and process parameters: the alloy obtained by the present invention can achieve a better modification effect, inhibit gas absorption, avoid stress release, self-quenching, casting deformation, and effectively reduce the probability and number of pores in the casting. These include: first, the present invention transforms the morphology of eutectic Si from slender needles to point rods, and reduces the average size from ~20-25μm to ~1-1.12μm; second, the precipitation of AlSi(Ti,Zr) in the alloy xPhase, which can become the nucleation core of the primary α-Al phase, can refine the primary α-Al grains, achieve fine grain strengthening, and enhance the aluminum-silicon alloy modification effect, wherein the average size of the primary α-Al grains is reduced from ~500-600μm to ~200-250μm, and the coarse α-AlSiFeMn phase is transformed into a finer and more evenly distributed α-AlSiFeMn phase, with the average size of α-AlSiFeMn reduced from ~25-30μm to ≤15μm. The finer phase can avoid stress concentration during deformation, thereby improving the casting quality of the alloy; thirdly, it effectively makes the mechanical properties of the alloy more stable and simultaneously improves the strength and plasticity of the alloy. The alloy has a yield strength of ≥134MPa, a tensile strength of ≥271MPa, and an elongation of ≥12.5%; and is suitable for large-scale production of large, complex, and irregularly shaped components with large wall thickness differences. DETAILED DESCRIPTION
[0021] In order to make the objectives, technical solutions and effects of the present invention clearer and more specific, the present invention is further described in detail in the following examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of protection of the claims of the present invention.
[0022] The raw materials used in the following examples and comparative examples are 99.75% aluminum, 99.99% magnesium, Al-20Si, Al-10Mn master alloy, Al-10Sr master alloy, Al-10Ce master alloy, Al-10Zr master alloy, and Al-10Ti master alloy.
[0023] Example 1
[0024] A high-strength and plastic casting hypoeutectic aluminum-silicon alloy 1 is composed of the following components, calculated by mass percentage: Si: 9.0 wt.%, Mg: 0.20 wt.%, Mn: 0.30 wt.%, Sr: 0.05 wt.%, Ce: 0.03 wt.%, Zr: 0.10 wt.%, Ti: 0.10 wt.%, with the inevitable impurity content being ≤ 0.2 wt.%, and the balance being Al. The high-strength and plastic casting hypoeutectic aluminum-silicon alloy 1 is prepared by the following method steps:
[0025] Step 1: Melt pure aluminum ingot, Al-20Si master alloy, and Al-10Mn master alloy at 780°C and let stand for 30 minutes; then add Mg, Al-10Zr master alloy, and Al-10Ti master alloy in sequence at 720°C, stir evenly, and let stand for 20 minutes to obtain aluminum-silicon alloy melt 1;
[0026] Step 2: Add Al-10Ce master alloy and Al-10Sr master alloy to the aluminum-silicon alloy melt 1 obtained in step 1 at 720° C., stir evenly, and let stand for 10 minutes to obtain aluminum-silicon alloy melt 2;
[0027] Step 3: heating the aluminum-silicon alloy melt 2 obtained in step 2 to 740° C., wrapping the refining agents C2Cl6 and KF with aluminum foil, pressing the refining agents C2Cl6 and KF to the bottom of the melt 2 with a pressure cover, stirring for 4 minutes, and standing for 9 minutes to obtain an aluminum-silicon alloy melt 3 (the mass ratio of C2Cl6 and KF is 2:1, and the mass ratio of C2Cl6 and KF in the aluminum-silicon alloy melt 3 is 0.3%);
[0028] Step 4: Cooling the aluminum-silicon alloy melt 3 obtained in step 3 to 720° C., introducing high-purity argon gas, performing degassing and impurity-refining treatment, and keeping the temperature for 6 minutes to obtain an aluminum-silicon alloy melt 4;
[0029] Step 5: The aluminum-silicon alloy melt 4 obtained in step 4 is poured into a water-cooled copper mold for sub-rapid solidification at 700°C with a sub-rapid solidification rate of 230°C / s to obtain a high-strength and plastic casting hypoeutectic aluminum-silicon alloy 1.
[0030] Example 2
[0031] A high-strength and plastic casting hypoeutectic aluminum-silicon alloy 2 is composed of the following components, calculated by mass percentage: Si: 8.0 wt.%, Mg: 0.25 wt.%, Mn: 0.20 wt.%, Sr: 0.07 wt.%, Ce: 0.04 wt.%, Zr: 0.12 wt.%, Ti: 0.10 wt.%, with the inevitable impurity content being ≤ 0.2 wt.%, and the balance being Al. The high-strength and plastic casting hypoeutectic aluminum-silicon alloy 2 is prepared by the following method steps:
[0032] Step 1: Melt pure aluminum ingot, Al-20Si master alloy, and Al-10Mn master alloy at 790°C and let stand for 40 minutes; then add Mg, Al-10Zr master alloy, and Al-10Ti master alloy in sequence at 730°C, stir evenly, and let stand for 25 minutes to obtain aluminum-silicon alloy melt 1;
[0033] Step 2: Cool the aluminum-silicon alloy melt 1 obtained in step 1 to 720° C., add Al-10Ce master alloy and Al-10Sr master alloy, stir evenly, and let stand for 15 minutes to obtain aluminum-silicon alloy melt 2;
[0034] Step 3: heating the aluminum-silicon alloy melt 2 obtained in step 2 to 745° C., wrapping the refining agents C2Cl6 and KF with aluminum foil, pressing the refining agents C2Cl6 and KF to the bottom of the melt 2 with a pressure cover, stirring for 5 minutes, and standing for 7 minutes to obtain an aluminum-silicon alloy melt 3 (the mass ratio of C2Cl6 and KF is 2:1, and the mass ratio of C2Cl6 and KF in the aluminum-silicon alloy melt 3 is 0.5%);
[0035] Step 4: Cooling the aluminum-silicon alloy melt 3 obtained in step 3 to 730° C., introducing high-purity argon gas, performing degassing and impurity-refining treatment, and keeping the temperature for 10 minutes to obtain an aluminum-silicon alloy melt 4;
[0036] Step 5: The aluminum-silicon alloy melt 4 obtained in step 4 is injected into a water-cooled copper mold for sub-rapid solidification at 705°C with a sub-rapid solidification rate of 160°C / s to obtain a high-strength and plastic casting hypoeutectic aluminum-silicon alloy 2.
[0037] Example 3
[0038] The high-strength and plastic casting hypoeutectic aluminum-silicon alloy 3 is composed of the following components, calculated by mass percentage: Si: 7.5 wt.%, Mg: 0.40 wt.%, Mn: 0.20 wt.%, Sr: 0.06 wt.%, Ce: 0.05 wt.%, Zr: 0.09 wt.%, Ti: 0.11 wt.%, and the inevitable impurity content is ≤ 0.2 wt.%, with the balance being Al. The high-strength and plastic casting hypoeutectic aluminum-silicon alloy 3 is prepared by the following method steps:
[0039] Step 1: Melt pure aluminum ingot, Al-20Si master alloy, and Al-10Mn master alloy at 800°C and let stand for 50 minutes; then add Mg, Al-10Zr master alloy, and Al-10Ti master alloy in sequence at 720°C, stir evenly, and let stand for 30 minutes to obtain aluminum-silicon alloy melt 1;
[0040] Step 2: Add Al-10Ce master alloy and Al-10Sr master alloy to the aluminum-silicon alloy melt 1 obtained in step 1 at 730° C., stir evenly, and let stand for 25 minutes to obtain aluminum-silicon alloy melt 2;
[0041] Step 3: heating the aluminum-silicon alloy melt 2 obtained in step 2 to 750° C., wrapping the refining agents C2Cl6 and KF with aluminum foil, pressing the refining agents C2Cl6 and KF to the bottom of the melt 2 with a pressure cover, stirring for 7 minutes, and standing for 10 minutes to obtain an aluminum-silicon alloy melt 3 (the mass ratio of C2Cl6 and KF is 2:1, and the mass ratio of C2Cl6 and KF in the aluminum-silicon alloy melt 3 is 0.7%);
[0042] Step 4: Cooling the aluminum-silicon alloy melt 3 obtained in step 3 to 725° C., introducing high-purity argon gas, performing degassing and impurity-refining treatment, and keeping the temperature for 8 minutes to obtain an aluminum-silicon alloy melt 4;
[0043] Step 5: The aluminum-silicon alloy melt 4 obtained in step 4 is poured into a water-cooled copper mold for sub-rapid solidification at 710°C with a sub-rapid solidification rate of 200°C / s to obtain a high-strength and plastic casting hypoeutectic aluminum-silicon alloy 3.
[0044] Example 4
[0045] The high-strength and plastic casting hypoeutectic aluminum-silicon alloy 4 is composed of the following components, calculated by mass percentage: Si: 7.0 wt.%, Mg: 0.30 wt.%, Mn: 0.30 wt.%, Sr: 0.07 wt.%, Ce: 0.05 wt.%, Zr: 0.11 wt.%, Ti: 0.12 wt.%, and the inevitable impurity content is ≤ 0.2 wt.%, with the balance being Al. The high-strength and plastic casting hypoeutectic aluminum-silicon alloy 4 is prepared by the following method steps:
[0046] Step 1: Melt pure aluminum ingot, Al-20Si master alloy, and Al-10Mn master alloy at 785°C and let stand for 60 minutes; then add Mg, Al-10Zr master alloy, and Al-10Ti master alloy in sequence at 725°C, stir evenly, and let stand for 30 minutes to obtain aluminum-silicon alloy melt 1;
[0047] Step 2: Add Al-10Ce master alloy and Al-10Sr master alloy to the aluminum-silicon alloy melt 1 obtained in step 1 at 720° C., stir evenly, and let stand for 25 minutes to obtain aluminum-silicon alloy melt 2;
[0048] Step 3: heating the aluminum-silicon alloy melt 2 obtained in step 2 to 755° C., wrapping the refining agents C2Cl6 and KF with aluminum foil, pressing the refining agents C2Cl6 and KF to the bottom of the melt 2 with a pressure cover, stirring for 6 minutes, and standing for 15 minutes to obtain an aluminum-silicon alloy melt 3 (the mass ratio of C2Cl6 and KF is 2:1, and the mass ratio of C2Cl6 and KF in the aluminum-silicon alloy melt 3 is 1.0%);
[0049] Step 4: Cooling the aluminum-silicon alloy melt 3 obtained in step 3 to 730° C., introducing high-purity argon gas, performing degassing and impurity-refining treatment, and keeping the temperature for 10 minutes to obtain an aluminum-silicon alloy melt 4;
[0050] Step 5: The aluminum-silicon alloy melt 4 obtained in step 4 is injected into a water-cooled copper mold for sub-rapid solidification at 707°C with a sub-rapid solidification rate of 240°C / s to obtain a high-strength plastic casting hypoeutectic aluminum-silicon alloy 4.
[0051] Comparative Example 1
[0052] He Bing, Qin Ming, Huang Bei, et al. "Effect of Sc and Y Composite Effect on Microstructure and Properties of A356 Alloy[J]. Special Casting and Nonferrous Alloys, 2017, 37(12):1385-1389. DOI:10.15980 / j.tzzz.2017.12.030. The report mentioned an A356-0.2Sc-0.2Y alloy. The commercial A356 alloy consists of the following components in terms of mass percentage: Si: 7.5wt.%, Mg: 0.30wt.%, Ti≤0.2wt.%, Fe≤0.12wt.%, Mn≤0.05wt.%, Cu≤0.1wt.%, Zn≤0.05wt.%, Sc: 0.2%; Y: 0.2%, the balance is Al. The cast alloy is heat treated at 540℃×4h and then at 155℃×10h to obtain an alloy with a tensile strength of 258MPa and an elongation of 4.7%.
[0053] Comparative Example 2
[0054] Tian Zhanfeng, Ge Sujing, Yuan Gaoli, et al. A renewable high-strength and tough heat-treatment-free aluminum alloy and its preparation method and die-casting process [P]. Hebei Province: CN202311414034.0, 2024-05-14. The patent reports a die-cast Al-8.65Si-0.35Fe-0.38Mn-0.15Mg-0.93Cu-0.4Zn-0.018Sr-0.04Cr-0.02Ni aluminum alloy, which is cast by vacuum high-pressure casting with a casting pressure of 1400 bar, a slow shot speed of 0.4 m / s; a fast shot speed of 3.5 m / s; a mold temperature and a barrel temperature of 200°C; a flat mold with a length of 200 mm and a width of 65 mm and a wall thickness of 3 mm; and a vacuum degree of the vacuum machine cavity of <50 mbar. The alloy obtained has a tensile strength of 270 MPa, a yield strength of 122 MPa, and an elongation of 10.2%.
[0055] Comparative Example 3
[0056] The cast hypoeutectic aluminum-silicon alloy is composed of the following components in percentage by mass: Si: 5.8 wt.%, Mg: 0.09 wt.%, Mn: 0.08 wt.%, Sr: 0.015 wt.%, Ce: 0.01 wt.%, Zr: 0.07 wt.%, Ti: 0.07 wt.%, unavoidable impurity content ≤ 0.2 wt.%, and the balance is Al. The cast hypoeutectic aluminum-silicon alloy is prepared by the following method steps:
[0057] Step 1: Melt pure aluminum ingot, Al-20Si master alloy, and Al-10Mn master alloy at 755°C and let stand for 19 minutes; then add Mg, Al-10Zr master alloy, and Al-10Ti master alloy in sequence at 697°C, stir evenly, and let stand for 9 minutes to obtain aluminum-silicon alloy melt 1;
[0058] Step 2: Add Al-10Ce master alloy and Al-10Sr master alloy to the aluminum-silicon alloy melt 1 obtained in step 1 at 695° C., stir evenly, and let stand for 4 minutes to obtain aluminum-silicon alloy melt 2;
[0059] Step 3: heating the aluminum-silicon alloy melt 2 obtained in step 2 to 725° C., wrapping the refining agents C2Cl6 and KF with aluminum foil, pressing the refining agents C2Cl6 and KF to the bottom of the melt 2 with a pressure cover, stirring for 2 minutes, and standing for 4 minutes to obtain an aluminum-silicon alloy melt 3 (the mass ratio of C2Cl6 and KF is 1:1, and the mass ratio of C2Cl6 and KF in the aluminum-silicon alloy melt 3 is 0.1%).
[0060] Step 4: Cooling the aluminum-silicon alloy melt 3 obtained in step 3 to 700° C., introducing high-purity argon gas, performing degassing and impurity removal refining treatment, and keeping the temperature for 4 minutes to obtain an aluminum-silicon alloy melt 4;
[0061] Step 5: The aluminum-silicon alloy melt 4 obtained in step 4 is injected into a water-cooled copper mold for sub-rapid solidification at 685°C with a sub-rapid solidification rate of 75°C / s to obtain a cast hypoeutectic aluminum-silicon alloy.
[0062] Table 1 is a comparison of the mechanical properties of the alloys obtained in Examples 1-4 and Comparative Examples 1-3
[0063]
[0064] Compared with existing technologies, this invention reduces alloy production costs, expands the applicability of the alloy, and significantly improves the strength and plasticity of the alloy by reducing the number and amount of alloying elements added, eliminating the need for high-temperature, long-term heat treatment, simplifying the processing, and shortening the preparation process. This approach, while focusing on practical production and application, significantly improves the alloy's strength and plasticity. By synergistically regulating the interactions between alloy components, proportions, processes, and process parameters, this invention develops a low-cost alloy with excellent refinement and modification effects, achieving a yield strength of 134 MPa or greater, a tensile strength of 271 MPa or greater, and an elongation of 12.5% or greater.
[0065] Compared to the present invention, Comparative Example 1 added high contents of the relatively expensive rare earth elements Sc and Y, and also incorporated heat treatment processes such as high-temperature solutionization and aging. The resulting aluminum alloy exhibited a tensile strength of 258 MPa and an elongation of 4.7%. While prior art reports suggest that the addition of high rare earth contents and heat treatment processes can improve the mechanical properties of alloys, the minimum strength and ductility of the alloys in the present invention's examples were higher than those of the alloy obtained in Comparative Example 1.
[0066] Compared with the present invention, Comparative Example 2 added a variety of alloying elements at high concentrations, resulting in high cost. It also used a complex and costly high-pressure die-casting process. The aluminum alloy obtained in Comparative Example 2 had a tensile strength of 270 MPa and an elongation of 10.2%. The strength and ductility of the alloy obtained in Comparative Example 2 were lower than the minimum strength and ductility of the alloy obtained in the examples of the present invention. This demonstrates that the present invention achieves simultaneous improvements in alloy strength and ductility while reducing the number and concentration of alloying elements and simplifying the process.
[0067] The components and processes used in the present invention are the same as those in Comparative Example 3, but the component ratios and process parameters of Comparative Example 3 are not within the scope of protection of the claims of the present invention. As a result, the strength and plasticity of the alloys obtained in Comparative Example 3 are lower than the minimum strength and plasticity of the alloys obtained in the embodiments of the present invention. This shows that only within the scope of protection of the claims of the present invention can the simultaneous improvement of the strength and plasticity of the alloys be achieved.
[0068] Compared with the prior art, the present invention omits the addition of high-content precious rare earths (the Sc and other components added in the prior art are relatively expensive among rare earths), high-temperature and long-term heat treatment processes, complex casting processes, and reduces the types and contents of added raw materials, while simultaneously improving the strength and plasticity of the alloy; the present invention reduces production costs and simplifies the process by regulating the interaction between components, component ratios, and process parameters, and only within the scope of protection of the claims of the present invention can the strength and plasticity of the alloy be simultaneously improved, making it suitable for industrial production.
Claims
1. A heat-treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy, characterized in that: According to mass percentage, it consists of the following components composition: Si: 6.0-10.0wt.%, Mg: 0.10-0.50wt.%, Mn: 0.10-0.50wt.%, Sr: 0.02-0.09wt.%, Ce: 0.02-0.06wt.%, Zr: 0.08-0.14wt.%, Ti: 0.08-0.14wt.%, inevitable impurity content ≤0.2wt.%, balance Al; the preparation method of the alloy comprises the following steps: Step 1: melt pure aluminum ingot, Al-20Si master alloy, and Al-10Mn master alloy at 760-810° C., and stand for 20-70 minutes; add pure Mg, Al-10Zr master alloy, and Al-10Ti master alloy in sequence at 700-740° C., stir evenly, and stand for 10-50 minutes to obtain aluminum-silicon alloy melt 1; Step 2: Add Al-10Ce master alloy and Al-10Sr master alloy to the aluminum-silicon alloy melt 1 obtained in step 1 at 700-740° C., stir evenly, and stand for 5-30 minutes to obtain an aluminum-silicon alloy melt 2; Step 3: heating the aluminum-silicon alloy melt 2 obtained in step 2 to 730-770° C., wrapping the refining agent C2Cl6 and KF with aluminum foil, pressing the refining agent C2Cl6 and KF to the bottom of the melt 2 with a pressure cover, stirring for 3-10 minutes, and standing for 5-20 minutes to obtain an aluminum-silicon alloy melt 3; Step 4: cool the aluminum-silicon alloy melt 3 obtained in step 3 to 710-740° C., introduce high-purity argon gas, perform degassing and impurity removal refining treatment, and keep the temperature for 5-15 minutes to obtain an aluminum-silicon alloy melt 4; Step 5: injecting the aluminum-silicon alloy melt 4 obtained in step 4 into a water-cooled copper mold at 690-720° C. for sub-rapid solidification to obtain a heat-treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy, wherein the sub-rapid solidification is: a sub-rapid solidification rate of 80-450° C. / s; The mass ratio of C2Cl6 and KF in step 3 is 2:1 to 4:1; the mass ratio of C2Cl6 and KF in the aluminum-silicon alloy melt 3 is 0.2-1%.
2. The heat treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy according to claim 1, characterized in that: According to mass percentage, it consists of the following components composition: Si: 7.0~9.0wt.%, Mg: 0.20~0.40wt.%, Mn: 0.20~0.40wt.%, Sr: 0.05~0.07wt.%, Ce: 0.03~0.05wt.%, Zr: 0.09~0.12wt.%, Ti: 0.09~0.12wt.%, and the balance is Al.
3. The heat treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy according to claim 1, characterized in that: The pure aluminum ingot, Al-20Si master alloy, and Al-10Mn master alloy described in step 1 are melted at 780-800° C. and allowed to stand for 30-60 minutes; pure Mg, Al-10Zr master alloy, and Al-10Ti master alloy are added in sequence at 720-730° C., stirred evenly, and allowed to stand for 20-30 minutes to obtain an aluminum-silicon alloy melt 1.
4. The heat treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy according to claim 1, characterized in that: The aluminum-silicon alloy melt 1 described in step 2 is added with Al-10Ce master alloy and Al-10Sr master alloy at 720-730° C. and allowed to stand for 10-25 minutes to obtain an aluminum-silicon alloy melt 2.
5. The heat treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy according to claim 1, characterized in that: Step 3 describes heating the aluminum-silicon alloy melt 2 to 740-760°C, wrapping the refining agents C2Cl6 and KF with aluminum foil, pressing the refining agents C2Cl6 and KF to the bottom of the melt 2 with a pressure cover, stirring for 4-7 minutes, and standing for 6-15 minutes.
6. The heat treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy according to claim 1, characterized in that: Step 4 is to cool the aluminum-silicon alloy melt 3 to 720-730° C., introduce high-purity argon gas, perform degassing and impurity removal refining treatment, and keep the temperature for 6-10 minutes.
7. The heat treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy according to claim 1, characterized in that: The aluminum-silicon alloy melt 4 described in step 5 is injected into a water-cooled copper mold at 700-710° C. for sub-rapid solidification to obtain a high-strength plastic casting hypoeutectic aluminum-silicon alloy.
8. The heat treatment-free high-strength plastic casting hypoeutectic aluminum-silicon alloy according to claim 1, characterized in that: The sub-rapid solidification rate in step 5 is 100-300°C / s.
Citation Information
Cited By
Cu-Zn-Ti-Si alloy synergistically strengthened by primary phase and hypoeutectic structure and preparation method for regulating components and cooling speed of Cu-Zn-Ti-Si alloy
CN121250175A