Refractory high-entropy alloy with excellent corrosion resistance and preparation method thereof

By adjusting the proportion of Ti, Cr, Zr, Ta, W element and smelting process, Ti35Cr10Zr15Ta25W15 high-entropy alloy was prepared, which solved the problem of insufficient corrosion performance of traditional alloys in marine environments and achieved excellent corrosion resistance under ocean and high temperature conditions Performance, suitable for marine ships and aerospace fields.

CN118880152APending Publication Date: 2024-11-01HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078339.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional alloys have insufficient corrosion performance in marine environments, especially in high temperature conditions, and the uneven distribution of Cr elements leads to a decrease in corrosion resistance, which is difficult to meet the needs of aerospace, nuclear energy and ships.

Method used

Refractory high-entropy alloy composed of Ti, Cr, Zr, Ta, W and other elements. By adjusting the element ratio and multiple smelting to ensure the uniformity of the alloy, Ti35Cr10Zr15Ta25W15 high-entropy alloy with excellent corrosion resistance was prepared, using vacuum non-self Arc-consuming smelting technology and argon protection atmosphere.

Benefits of technology

In marine-like environments, Ti35Cr10Zr15Ta25W15 high-entropy alloy exhibits excellent corrosion resistance, with a pitting potential greater than twice that of 304L stainless steel, with a high melting point and passivation phenomenon, and is suitable for marine ships and aerospace fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880152A_ABST
    Figure CN118880152A_ABST
Patent Text Reader

Abstract

The invention discloses a refractory high-entropy alloy with excellent corrosion resistance and a preparation method of the refractory high-entropy alloy, and the refractory high-entropy alloy comprises corrosion-resistant elements of titanium and chromium and also comprises refractory elements of tungsten, tantalum and zirconium. The refractory high-entropy alloy disclosed by the invention has excellent corrosion resistance in a marine-like environment, namely a 3.5 wt.% NaCl solution at 25 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal materials and preparation thereof, and in particular to a refractory high entropy alloy with excellent corrosion resistance and a preparation method thereof. Background Art

[0002] The concept of high entropy alloy was first proposed by scholar Ye Junwei, who defined it as a material composed of five or more elements with each element accounting for 5at.% to 35at.%. As a new type of metal material, high entropy alloy has more outstanding properties than traditional alloys, such as high strength, high hardness, high plasticity, excellent corrosion resistance, and radiation resistance, by virtue of its unique design concept and four effects, namely "high entropy effect", "hysteresis diffusion effect", "lattice distortion effect" and "cocktail effect". Refractory high entropy alloys can be prepared by adding refractory metals such as Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W to high entropy alloys. This type of alloy inherits the performance advantages of high entropy alloys and refractory metals, which further expands its application scope and shows great application potential in aerospace, nuclear energy, ocean, shipbuilding and other fields.

[0003] In the marine environment, materials with excellent corrosion resistance are key materials for future applications in the field of marine ships. According to surveys, the economic losses caused by corrosion each year account for an average of more than 3% of the annual GDP of each country. Corrosion not only causes huge losses to the national economy, but also has a significant impact on people's safety, health and quality of life. 304 stainless steel is a commonly used corrosion-resistant alloy material, which is widely used in automobiles, medical equipment, building materials and marine ships. However, in stainless steel, due to the uneven distribution of Cr elements, carbides and σ phases in the alloy will deteriorate the corrosion resistance of the alloy and cause local corrosion of the alloy. In addition, alloys in high-temperature working environments need to have better corrosion resistance. Since traditional alloys have poor high-temperature resistance, high temperatures will aggravate the corrosion of alloys. In order to meet the needs of economic development, new corrosion-resistant materials need to be developed. Refractory high-entropy alloys are different from traditional alloys in design concepts, so that they can obtain alloy materials with special properties through composition design, regulation of different principal elements and phase organization design, and high-temperature resistance, which are expected to be used in aerospace, nuclear energy, ocean and shipbuilding industries.

[0004] Therefore, the development of refractory high-entropy alloys with excellent corrosion resistance is of great significance to the development of industries such as aerospace, nuclear energy, ocean and shipbuilding. Summary of the invention

[0005] Based on the problems existing in the above-mentioned prior art, the present invention provides a refractory high entropy alloy having excellent corrosion resistance in a marine-like environment, i.e., a 3.5wt.% NaCl solution at 25°C, and aims to adjust the proportion of each element so that the obtained refractory high entropy alloy exhibits excellent corrosion resistance in a marine-like environment.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] A refractory high entropy alloy with excellent corrosion resistance, characterized in that: its constituent elements include corrosion-resistant elements titanium and chromium, as well as refractory elements tungsten, tantalum, and zirconium; its composition is (Ti 7 Cr 2 Zr 3 Ta 5 ) x W y , where x+y=100, x=80~90, y=10~20, x is the atomic percentage of the sum of the four elements Ti, Cr, Zr, and Ta, and y is the atomic percentage of W.

[0008] The present invention (Ti 7 Cr 2 Zr 3 Ta 5 ) x W y A method for preparing a refractory high entropy alloy comprises the following steps:

[0009] Step 1, taking Ti, Cr, Zr, Ta and W metal raw materials, using a file and sandpaper to polish the metal surface to remove the surface oxide layer and attached impurities, placing the polished metal raw materials in ethanol for ultrasonic cleaning and drying; weighing each raw material according to the ratio;

[0010] Step 2: Place the prepared raw materials in the crucible of the vacuum non-consumable arc melting equipment in order from low to high melting points; evacuate the equipment to 8×10 -4 Pa, and argon is filled as a protective gas and the pressure in the melting chamber reaches -0.05MPa;

[0011] Step 3, arc is struck by a tungsten needle. After arc is struck, the titanium ingot is first melted to consume the residual oxygen in the furnace chamber, and then the metal raw material is melted; the alloy is melted multiple times to ensure that the total time the alloy is in liquid state during melting is not less than 60 minutes, and after a single melting, the alloy is turned over with a turning spoon to ensure the preparation of a uniform alloy; after the melting is completed, Ti is obtained. 35 Cr 10 Zr 15 Ta 25 W 15 Refractory high entropy alloys.

[0012] Preferably, in step 1, the purity of the Ti, Cr, Zr, Ta and W metal raw materials is not less than 99.99%.

[0013] Preferably, in step 1, the weighing is accurate to ±0.001 g.

[0014] Preferably, in step 3, the arc striking current is 18-20A, the current is adjusted to 160A-180A when melting titanium ingots, and the current is adjusted to 240A-280A when melting metal raw materials.

[0015] The beneficial effects of the present invention are as follows:

[0016] 1. The present invention is composed of five refractory metal elements: Ti, Cr, Zr, Ta, and W (Ti 7 Cr 2 Zr 3 Ta 5 ) x W y Refractory high entropy alloys have excellent corrosion resistance in marine environments; electrochemical tests have shown that Ti 35 Cr 10 Zr 15 Ta 25 W 15 The pitting potential of the refractory high entropy alloy in 3.5wt.% NaCl solution at 25°C is about twice that of 304L stainless steel, and it has a tertiary passivation phenomenon. The width of the passivation zone is much larger than that of 304L stainless steel, and the passivation current density is lower than that of 304L stainless steel, indicating that it has excellent corrosion resistance.

[0017] 2. The metal elements used in the refractory high entropy alloy of the present invention include corrosion-resistant elements titanium and chromium, which makes it have great application potential in the fields of ocean and shipbuilding.

[0018] 3. The refractory high entropy alloy of the present invention uses all refractory elements, which ensures that the alloy has excellent corrosion resistance while also having a high melting point, making it have good application prospects in the fields of aerospace, nuclear energy, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Ti obtained in Example 1 of the present invention 35 Cr 10 Zr 15 Ta 25 W 15 XRD patterns of the alloy.

[0020] Figure 2 Ti obtained in Example 1 of the present invention 35 Cr 10 Zr 15 Ta25 W 15 Potentiodynamic polarization curves of alloy and 304L stainless steel in 3.5wt.% NaCl solution at 25℃. DETAILED DESCRIPTION

[0021] In order to make the above-mentioned objects, features and advantages of the present invention more clear and explicit, the following is a summary of the present invention. Figure 1 and Figure 2 The specific implementation methods of the present invention are described in detail. The following content is only an example and explanation of the concept of the present invention. The technicians in this technical field can make various modifications or supplements to the specific implementation cases described or replace them with similar methods. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0022] The Ti prepared in the following examples 35 Cr 10 Zr 15 Ta 25 W 15 Refractory high entropy alloys are obtained by the following steps:

[0023] Step 1: Take Ti, Cr, Zr, Ta and W metal raw materials, use a file and sandpaper to polish the metal surface to remove the surface oxide layer and attached impurities, place the polished metal raw materials in ethanol for ultrasonic cleaning and drying; weigh each raw material according to the ratio, and weigh to an accuracy of ±0.001g.

[0024] Step 2: Place the prepared raw materials in the crucible of the vacuum non-consumable arc melting equipment in order from low to high melting points; evacuate the equipment to 8×10 -4 Pa, and argon is filled as a protective gas to make the smelting chamber pressure reach -0.05MPa.

[0025] Step 3: Adjust the current to 20A, and start the arc through the tungsten needle. Then adjust the current to 170A to melt the titanium ingot to consume the residual oxygen in the furnace chamber, and then adjust the current to 250A to melt the metal raw materials in the crucible. Melt the alloy multiple times according to the above method to ensure that the total time the alloy is in liquid state during melting is not less than 60 minutes. After a single melting, use a turning spoon to turn the alloy over to ensure that a uniform alloy is prepared. After the melting is completed, Ti is obtained. 35 Cr 10 Zr 15 Ta 25 W 15 Refractory high entropy alloys.

[0026] Example 1

[0027] Ti of this embodiment35 Cr 10 Zr 15 Ta 25 W 15 The atomic percentages of the refractory high entropy alloy, namely Ti, Cr, Zr, Ta and W, are 35 at.%, 10 at.%, 15 at.%, 25 at.% and 15 at.%, respectively.

[0028] Figure 1 Ti obtained in this example 35 Cr 10 Zr 15 Ta 25 W 15 The XRD pattern of the alloy shows that the alloy phase is composed of a single BCC phase.

[0029] Figure 2 Ti is obtained in this example 35 Cr 10 Zr 15 Ta 25 W 15 Potentiodynamic polarization curves of Ti alloy and 304L stainless steel in 3.5wt.%NaCl solution at 25℃ 35 Cr 10 Zr 15 Ta 25 W 15 The alloy has a tertiary passivation phenomenon and the pitting potential is 1.12V SCE The pitting potential of 304L stainless steel is about 0.49V SCE The results showed that Ti 35 Cr 10 Zr 15 Ta 25 W 15 The pitting potential of the alloy is about twice that of 304L stainless steel, the width of the passivation zone is much larger than that of 304L stainless steel, and the passivation current density is lower than that of 304L stainless steel, indicating that it has excellent corrosion resistance.

[0030] The above are merely exemplary embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A refractory high entropy alloy with excellent corrosion resistance, characterized by: The refractory high entropy alloy is a five-element single-phase alloy with the composition (Ti7Cr2Zr3Ta5) x W y , where x+y=100, x=80~90, y=10~20, x is the atomic percentage of the sum of the four elements Ti, Cr, Zr, and Ta, and y is the atomic percentage of W.

2. A method for preparing the refractory high entropy alloy according to claim 1, characterized in that: The steps include: Step 1: Take Ti, Cr, Zr, Ta, and W metal raw materials, polish the metal surfaces with a file and sandpaper to remove the surface oxide layer and attached impurities, ultrasonically clean the polished metal raw materials in ethanol, and dry them; weigh each raw material according to the ratio; Step 2: Place the prepared raw materials into the crucible of the vacuum non-consumable arc melting equipment in order of melting point from low to high; evacuate the equipment to 8×10 -4 Pa, then fill in argon as a protective gas and make the smelting chamber pressure reach -0.05MPa; Step 3: Use a tungsten needle to strike the arc. After striking the arc, melt the titanium ingot first to consume the residual oxygen in the furnace chamber, and then melt the metal raw materials; melt the alloy multiple times to ensure that the total time the alloy is in liquid state during melting is not less than 60 minutes, and use a turning spoon to turn the alloy over after each melting to ensure that a uniform alloy is prepared. After the smelting is completed, (Ti7Cr2Zr3Ta5) is obtained x W y Refractory high entropy alloys.

3. The preparation method according to claim 2, wherein: In step 1, the purity of the Ti, Cr, Zr, Ta, and W metal raw materials is not less than 99.99%.

4. The preparation method according to claim 2, wherein: In step 1, weigh to an accuracy of ±0.001g.

5. The preparation method according to claim 2, wherein: In step 3, the arc striking current is 18-20A. When melting titanium ingots, the current is adjusted to 160A-180A. When melting metal raw materials, the current is adjusted to 240A-280A.