Method for improving room-temperature tensile plasticity of refractory high-entropy alloy

By adjusting the component ratio and thermal isostatic pressing + heat treatment process of AlCrNbMoTaTiHf high-entropy alloy, the problem of insufficient room temperature plasticity is solved, significantly improving room temperature tensile plasticity and optimizing process efficiency.

CN118880153AActive Publication Date: 2024-11-01AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411165837.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-01
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Refractory high-entropy alloys such as AlCrNbMoTaTiHf are inadequate plasticity at room temperature, and existing component regulation and heat treatment methods cannot effectively improve their room temperature tensile plasticity.

Method used

By adjusting the component ratio and combining thermal isostatic pressure and thermal treatment synchronous treatment, the composition and process of AlCrNbMoTaTiHf high-entropy alloy are optimized, the content of Cr, Al, Mo and Hf elements are controlled, and the thermal isostatic pressure and low-temperature high-temperature redissolution are performed. The treatment is to close the internal defects and enhance the precipitation of the Hf-rich phase.

Benefits of technology

The room temperature tensile plasticity of cast AlCrNbMoTaTiHf high-entropy alloy was significantly improved, and the data increased from 11.8% to 15.9%, and the dispersion of the tensile plasticity data was reduced, with short process flow, high production efficiency and low energy consumption cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880153A_ABST
    Figure CN118880153A_ABST
Patent Text Reader

Abstract

The invention relates to a method for improving room-temperature tensile plasticity of a refractory high-entropy alloy, the refractory high-entropy alloy is an as-cast AlCrNbMoTaTiHf alloy, the method comprises the following steps: firstly, preliminarily obtaining AlCrNbMoTaTiHf refractory high-entropy alloy components with relatively good room-temperature plasticity by adjusting the component ratio, and then carrying out hot isostatic pressing and heat treatment synchronous treatment to obtain the refractory high-entropy alloy with good room-temperature plasticity. According to the technical scheme, through reasonable component design and matched hot isostatic pressing and heat treatment synchronous treatment, a new path is provided for improving the room-temperature tensile plasticity of the as-cast refractory high-entropy alloy, and the technical scheme is short in technological process, high in production efficiency and suitable for industrial production. The method is suitable for high-entropy alloy components formed in a direct as-cast state.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a method for improving room temperature tensile plasticity of a refractory high entropy alloy. The refractory high entropy alloy is a cast AlCrNbMoTaTiHf alloy and belongs to the technical field of metal materials. Background Art

[0002] Refractory high entropy alloys composed of refractory elements have excellent high temperature performance and other advantages. They are very promising new high temperature resistant metal materials. However, refractory high entropy alloys are typical BCC crystal structures and generally have the problem of insufficient room temperature plasticity. AlCrNbMoTaTiHf high entropy alloy is an important high temperature structural material among refractory high entropy alloys. In the future, it can be used as castings in high temperature resistant parts of aerospace. Similar to other refractory high entropy alloys, it also has the problem of insufficient room temperature plasticity.

[0003] At present, the main approach to improve the room temperature plasticity of refractory high entropy alloys is alloy composition regulation. In addition to composition regulation, plastic deformation and heat treatment are also important ways to improve the room temperature tensile plasticity of refractory high entropy alloys. However, the above measures cannot effectively improve the room temperature tensile plasticity of cast refractory high entropy alloys. Summary of the invention

[0004] In order to overcome the above technical deficiencies, the present invention provides a method for improving the room temperature tensile plasticity of a refractory high entropy alloy, and the refractory high entropy alloy targeted by the method is a cast AlCrNbMoTaTiHf alloy. The method firstly obtains an AlCrNbMoTaTiHf refractory high entropy alloy composition with relatively good room temperature plasticity by adjusting the component ratio, and then further improves the room temperature tensile plasticity of the cast refractory high entropy alloy by a method of simultaneous hot isostatic pressing and heat treatment.

[0005] To achieve the above purpose, the technical solution of the present invention is as follows:

[0006] The refractory high entropy alloy in the method for improving the room temperature tensile plasticity of the refractory high entropy alloy of the present invention is a cast AlCrNbMoTaTiHf alloy, and the molar expression of the AlCrNbMoTaTiHf alloy is Al a Cr b Nb c Mo d Ta e Ti f Hf g , where: a = 2 to 8, b = 2 to 6, c = 18 to 28, d = 4 to 9, e = 6 to 14, f = 30 to 40, g ≥ 15, 8 <a+b+d<16,a+b+c+d+e+f+g=100;

[0007] The technical solution of the invention firstly obtains the AlCrNbMoTaTiHf refractory high entropy alloy composition with good room temperature plasticity by adjusting the component ratio. The process of determining the above alloy composition is described as follows:

[0008] Previous studies have found that when the Al content in the AlCrNbMoTaTiHf refractory high entropy alloy exceeds 8at%, the Al element will cause the alloy lattice distortion to increase and easily precipitate the brittle phase A2, resulting in a significant decrease in the room temperature / high temperature plasticity of the high entropy alloy, especially the room temperature tensile plasticity as low as less than 0.5%. However, in order to ensure that the high entropy alloy has a certain antioxidant ability, the Al content was finally determined to be 2-8at%.

[0009] When the Cr element content in the high entropy alloy exceeds 6at%, the volume fraction of the Laves phase in the alloy exceeds 25%, and it aggregates into sheets, resulting in poor deformation coordination ability with the matrix. The room temperature tensile plasticity of the high entropy alloy is less than 2%. In order to ensure that the high entropy alloy has a certain antioxidant ability, the Cr element content is finally determined to be 2-6at%.

[0010] When the Mo element in the high-entropy alloy exceeds 9at%, the lattice distortion strengthening effect of the Mo element is too large, which causes a sharp drop in the continuous deformation ability of the matrix at room temperature, resulting in the high-entropy alloy having a room-temperature tensile plasticity of less than 4%; although reducing the Mo element content can improve the room-temperature plasticity of the alloy, when the Mo content is lower than 4at%, the lattice distortion strengthening effect brought by the Mo element is not obvious, resulting in the room-temperature strength of the high-entropy alloy being lower than 948MPa, so the Mo content is finally determined to be 4-9at%.

[0011] Previous studies have also found that if the Al, Cr and Mo contents are all taken to the upper limit (Al content is 8at%, Cr content is 6at%, Mo content is 9at%), the lattice distortion caused by the synergy of the three elements is stronger, resulting in the room temperature tensile plasticity of the refractory high entropy alloy being less than 5%. Further experimental research and verification have shown that when the sum of Al, Cr and Mo elements is not higher than 16at%, the refractory high entropy alloy can be guaranteed to have good room temperature tensile plasticity, and its average value is not less than 10%.

[0012] The influence of Hf element on the room temperature tensile plasticity of AlCrNbMoTaTiHf refractory high entropy alloy is also very significant. Previous studies have found that when the Hf element content is lower than 15at%, the room temperature tensile plasticity of the high entropy alloy is significantly reduced, and the elongation is less than 5%. On the contrary, when the Hf element is not less than 15at%, a high melting point white Hf-rich phase is precipitated in the high entropy alloy matrix. This precipitated phase can effectively disperse the stress concentration in the BCC matrix during room temperature tensile deformation, enhance deformation coordination, and thus significantly improve the room temperature tensile plasticity of the high entropy alloy. Therefore, the Hf element content in the refractory high entropy alloy should not be less than 15at%.

[0013] The technical solution of the present invention is directed to a preparation process of the AlCrNbMoTaTiHf alloy, which includes hot isostatic pressing and heat treatment performed simultaneously, and the process steps are as follows:

[0014] Step 1: According to the molar expression of the AlCrNbMoTaTiHf alloy, the molar percentage of each component is converted into weight percentage, the metal elements Al, Cr, Nb, Mo, Ta, Ti and Hf are weighed, and the metal raw materials are melted in an electromagnetic suspension melting furnace to obtain a high entropy alloy ingot, and then the alloy ingot is turned over and melted 3 to 6 times and slowly cooled to obtain a cast AlCrNbMoTaTiHf high entropy alloy ingot;

[0015] Step 2: Place the cast AlCrNbMoTaTiHf high entropy alloy ingot prepared in step 1 in a hot isostatic pressing device, first heat it to 600-800°C, keep it warm for 2-4 hours, then heat it to 1160-1250°C by increasing temperature and pressure, perform hot isostatic pressing at a pressure of not less than 100 MPa, and keep it warm for 1-2 hours;

[0016] Step 3: Then, the heating is stopped while maintaining the pressure, and the cast AlCrNbMoTaTiHf high entropy alloy ingot is slowly cooled to 1000-1050° C. in the furnace, and then the pressure is released and the ingot is rapidly cooled to room temperature.

[0017] Furthermore, the raw material purity of the metal elements Al, Cr, Nb, Mo, Ta, Ti and Hf in step 1 is greater than 99.9%.

[0018] Furthermore, the pressure range of the hot isostatic pressing in step 2 is 120 to 180 MPa.

[0019] Furthermore, the slow cooling rate along with the furnace in step 3 is 60-100° C. / h.

[0020] After the alloy composition optimization and experimental verification, the technical solution of the present invention has the material property of good room temperature tensile plasticity of AlCrNbMoTaTiHf high entropy alloy. However, there are internal casting defects in the refractory high entropy alloy ingot after melting and casting, and the casting defects are easily used as crack sources during the room temperature tensile process, resulting in premature fracture of the sample. Moreover, the size of the high entropy alloy ingot for experimental verification is relatively small, while the size of the high entropy alloy ingot for engineering is relatively large, which will inevitably lead to an increase in the number of internal defects in the ingot, an increase in the volume of internal defects in some areas, and thus an increase in the discreteness of the room temperature tensile plasticity data of large-size ingots. The hot isostatic pressing technology can close the internal defects of the cast refractory high entropy alloy to the greatest extent through the three-dimensional compressive stress under certain temperature, pressure and time, prevent premature fracture of the sample, and reduce the discreteness of the tensile plasticity data.

[0021] In addition to hot isostatic pressing technology, considering that the AlCrNbMoTaTiHf high entropy alloy with good room temperature plasticity has the characteristics of low melting point phase and high melting point phase, it is also necessary to match the corresponding heat treatment, that is, dissolve the low melting point phase in the low temperature section + dissolve the high melting point phase in the high temperature section 10 to 20 ° C higher than the high melting point phase, and then precipitate a relatively coarse high melting point Hf-rich phase through slow cooling after high temperature heat treatment. Only through the matching hot isostatic pressing + heat treatment process can the maximum potential of room temperature stretching of cast AlCrNbMoTaTiHf high entropy alloy materials be brought into play, achieving or even exceeding the expected effect of alloy composition design optimization.

[0022] The present invention performs hot isostatic pressing and heat treatment simultaneously, which can not only ensure that the refractory high entropy alloy undergoes corresponding heat treatment, but also effectively close the internal defects of the cast high entropy alloy, and can greatly improve the room temperature tensile plasticity of the cast high entropy alloy. The preliminary experimental results show that the room temperature tensile plasticity of the AlCrNbMoTaTiHf high entropy alloy after melt casting is 11.8%, and the room temperature tensile plasticity of the high entropy alloy of this composition after hot isostatic pressing and heat treatment is 15.9%. It can be seen that the room temperature tensile plasticity after hot isostatic pressing and heat treatment is improved by 34.7%.

[0023] In addition, the simultaneous hot isostatic pressing and heat treatment process has a short process, high production efficiency, and low energy consumption cost, providing a new path to further improve the room temperature tensile plasticity of cast AlCrNbMoTaTiHf high entropy alloy.

[0024] The beneficial technical effects of the technical solution of the present invention can be summarized as follows:

[0025] 1. The present invention controls the Cr element content to reduce the precipitation amount of harmful phases such as Laves in the matrix through reasonable composition design, controls the Al and Mo contents to improve the room temperature continuous deformation ability of the matrix, and increases the Hf element content to increase the content of the beneficial Hf-rich phase to enhance deformation coordination, thereby improving the room temperature tensile plasticity of the cast AlCrNbMoTaTiHf refractory high entropy alloy.

[0026] Second, the present invention uses a method of matching hot isostatic pressing and heat treatment simultaneously to close the internal defects of the cast refractory high entropy alloy to the greatest extent, and at the same time, it can increase the beneficial Hf-rich phase through low temperature + high temperature two-stage dissolution and slow cooling heat treatment, thereby improving the room temperature tensile plasticity of the cast high entropy alloy. The process method has a short process flow, high production efficiency, and low energy consumption cost, providing a new path for further improving the room temperature tensile plasticity of the cast AlCrNbMoTaTiHf high entropy alloy.

[0027] 3. The method of the present invention is also applicable to improving the room temperature tensile plasticity of other cast refractory high entropy alloy systems, and its hot isostatic pressing and heat treatment simultaneous treatment method is also applicable to improving the room temperature tensile plasticity of other laser additively processed refractory high entropy alloy systems. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The cast Al5Cr2Nb in Example 1 23 Mo6Ta9Ti 35 Hf 20 Room temperature tensile curves of refractory high entropy alloys.

[0029] Figure 2 The cast Al6Cr2Nb in Example 2 22 Mo5Ta8Ti 36 Hf 21 Room temperature tensile curves of refractory high entropy alloys.

[0030] Figure 3 The cast Al4Cr3Nb in Example 3 24 Mo6Ta8Ti 37 Hf 18 Room temperature tensile curves of refractory high entropy alloys.

[0031] Figure 4 For the implementation of the as-cast Al4Cr2Nb 24 Mo5Ta8Ti 35 Hf 22 Room temperature tensile curves of refractory high entropy alloys. DETAILED DESCRIPTION

[0032] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments:

[0033] Example 1

[0034] The process steps for preparing a cast AlCrNbMoTaTiHf refractory high entropy alloy with high room temperature tensile plasticity by using the technical solution of the present invention are as follows:

[0035] Step 1: In this embodiment, the molar expression of the cast refractory high entropy alloy is Al5Cr2Nb 23 Mo6Ta9Ti 35 Hf 20 According to the molar expression, the weight percentage of each component is: Al 1.4%, Cr 1.1%, Nb 21.7%, Mo 5.8%, Ta 16.6%, Ti 17.1%, Hf 36.3%; remove impurities on the surface of the metal element Al, Cr, Nb, Mo, Ta, Ti, Hf raw materials, use acetone ultrasonic cleaning, take out and dry for use;

[0036] Step 2: Place the weighed metal element into the electromagnetic suspension melting furnace and evacuate to 2.5×10 -3 After the Pa, high-purity argon gas is filled in for smelting. After the metal raw materials are melted, refractory high-entropy alloy ingots are obtained. Then, each furnace of alloy ingots is turned over and melted 4 times and slowly cooled to finally obtain cast Al5Cr2Nb 23 Mo6Ta9Ti 35 Hf 20 Refractory high entropy alloy ingots;

[0037] Step 3: Cast Al5Cr2Nb 23 Mo6Ta9Ti 35 Hf 20 The refractory high entropy alloy ingot is placed in a hot isostatic pressing device, first heated to 780°C with the furnace, kept warm for 3 hours, and then hot isostatically pressed at 1180°C and 150MPa with the furnace in a temperature and pressure increasing manner, and kept warm for 2 hours;

[0038] Step 4: Then stop heating under pressure holding and cast Al5Cr2Nb 23 Mo6Ta9Ti 35 Hf 20 The refractory high entropy alloy ingot is slowly cooled in the furnace at a rate of 100°C / h to 1020°C, then depressurized and rapidly cooled to room temperature.

[0039] The cast Al5Cr2Nb prepared in this embodiment 23 Mo6Ta9Ti 35 Hf 20 Tensile specimens were cut from refractory high entropy alloy ingots and tested for room temperature tensile properties using a universal tensile testing machine. The results are shown in Figure 2. Figure 1The room temperature tensile elongation of the cast refractory high entropy alloy is 23.5%, indicating that the room temperature tensile plasticity of the alloy is good.

[0040] Example 2

[0041] The process steps for preparing a cast AlCrNbMoTaTiHf refractory high entropy alloy with high room temperature tensile plasticity by using the technical solution of the present invention are as follows:

[0042] Step 1: In this embodiment, the molar expression of the cast refractory high entropy alloy is Al6Cr2Nb 22 Mo5Ta8Ti 36 Hf 21 According to the molar expression, the weight percentage of each component is: Al 1.7%, Cr 1.1%, Nb 21.0%, Mo4.9%, Ta 14.9%, Ti 17.8%, Hf 38.6%; remove impurities on the surface of the metal element Al, Cr, Nb, Mo, Ta, Ti, Hf raw materials, use acetone ultrasonic cleaning, take out and dry for use;

[0043] Step 2: Place the weighed metal element into the electromagnetic suspension melting furnace and evacuate to 2.5×10 -3 After the Pa, high-purity argon gas is filled in for smelting. After the metal raw materials are melted, refractory high-entropy alloy ingots are obtained. Then, each furnace of alloy ingots is turned over and melted three times and slowly cooled to finally obtain cast Al6Cr2Nb 22 Mo5Ta8Ti 36 Hf 21 Refractory high entropy alloy ingots;

[0044] Step 3: Cast Al6Cr2Nb 22 Mo5Ta8Ti 36 Hf 21 The refractory high entropy alloy ingot is placed in a hot isostatic pressing device, first heated to 750°C with the furnace, kept at this temperature for 2.5 hours, and then hot isostatically pressed at 1205°C and 140MPa with the furnace in a heating and pressure increasing manner, and kept at this temperature for 1.5 hours;

[0045] Step 4: Then stop heating under pressure and cast Al6Cr2Nb 22 Mo5Ta8Ti 36 Hf 21 The refractory high entropy alloy ingot is slowly cooled in the furnace at a rate of 60°C / h to 1000°C, then depressurized and rapidly cooled to room temperature.

[0046] The cast Al6Cr2Nb prepared in this example 22 Mo5Ta8Ti 36 Hf 21Tensile specimens were cut from refractory high entropy alloy ingots and tested for room temperature tensile properties using a universal tensile testing machine. The results are shown in Figure 2. Figure 2 The room temperature tensile elongation of the cast refractory high entropy alloy is 17.7%, indicating that the alloy has good room temperature tensile plasticity.

[0047] Example 3

[0048] The process steps for preparing a cast AlCrNbMoTaTiHf refractory high entropy alloy with high room temperature tensile plasticity by using the technical solution of the present invention are as follows:

[0049] Step 1: In this embodiment, the molar expression of the cast refractory high entropy alloy is Al4Cr3Nb 24 Mo6Ta8Ti 37 Hf 18 According to the molar expression, the weight percentage of each component is: Al 1.1%, Cr 1.6%, Nb 23.5%, Mo6.1%, Ta 15.2%, Ti 18.7%, Hf 33.8%; remove impurities on the surface of the metal single substance Al, Cr, Nb, Mo, Ta, Ti, Hf raw materials, use acetone ultrasonic cleaning, take out and dry for use;

[0050] Step 2: Place the weighed metal element into the electromagnetic suspension melting furnace and evacuate to 2.5×10 -3 After the Pa, high-purity argon gas is filled in for smelting. After the metal raw materials are melted, refractory high-entropy alloy ingots are obtained. Then, each furnace of alloy ingots is turned over and melted 5 times and slowly cooled to finally obtain cast Al4Cr3Nb 24 Mo6Ta8Ti 37 Hf 18 Refractory high entropy alloy ingots;

[0051] Step 3: Cast Al4Cr3Nb 24 Mo6Ta8Ti 37 Hf 18 The refractory high entropy alloy ingot is placed in a hot isostatic pressing device, first heated to 680°C with the furnace, kept at this temperature for 2 hours, and then hot isostatically pressed at 1190°C and 160MPa with the furnace in a heating and pressure increasing manner, and kept at this temperature for 1.5 hours;

[0052] Step 4: Then stop heating under pressure holding and cast Al4Cr3Nb 24 Mo6Ta8Ti 37 Hf 18 The refractory high entropy alloy ingot is slowly cooled in the furnace at a rate of 90°C / h to 1050°C, then depressurized and rapidly cooled to room temperature.

[0053] The cast Al4Cr3Nb prepared in this example24 Mo6Ta8Ti 37 Hf 18 Tensile specimens were cut from refractory high entropy alloy ingots and tested for room temperature tensile properties using a universal tensile testing machine. The results are shown in Figure 2. Figure 3 The room temperature tensile elongation of the cast refractory high entropy alloy is 20.4%, indicating that the alloy has good room temperature tensile plasticity.

[0054] Example 4

[0055] The process steps for preparing a cast AlCrNbMoTaTiHf refractory high entropy alloy with high room temperature tensile plasticity by using the technical solution of the present invention are as follows:

[0056] Step 1: In this embodiment, the molar expression of the cast refractory high entropy alloy is Al4Cr2Nb 24 Mo5Ta8Ti 35 Hf 22 According to the molar expression, the weight percentage of each component is: Al 1.1%, Cr 1.0%, Nb 22.4%, Mo4.8%, Ta 14.5%, Ti 16.8%, Hf 39.4%; remove impurities on the surface of the metal single substance Al, Cr, Nb, Mo, Ta, Ti, Hf raw materials, use acetone ultrasonic cleaning, take out and dry for use;

[0057] Step 2: Place the weighed metal element into the electromagnetic suspension melting furnace and evacuate to 2.5×10 -3 After the Pa, high-purity argon gas is filled in for smelting. After the metal raw materials are melted, refractory high-entropy alloy ingots are obtained. Then, each furnace of alloy ingots is turned over and melted three times and slowly cooled to finally obtain cast Al4Cr2Nb 24 Mo5Ta8Ti 35 Hf 22 Refractory high entropy alloy ingots;

[0058] Step 3: Cast Al4Cr2Nb 24 Mo5Ta8Ti 35 Hf 22 The refractory high entropy alloy ingot is placed in a hot isostatic pressing device, first heated to 700°C with the furnace, kept warm for 3 hours, and then hot isostatically pressed at 1220°C and 180MPa with the furnace in a temperature and pressure increasing manner, and kept warm for 1 hour;

[0059] Step 4: Then stop heating under pressure holding and cast Al4Cr2Nb 24 Mo5Ta8Ti 35 Hf 22 The refractory high entropy alloy ingot is slowly cooled in the furnace at a rate of 80°C / h to 1010°C, then depressurized and rapidly cooled to room temperature.

[0060] The cast Al4Cr2Nb prepared in this embodiment 24 Mo5Ta8Ti 35 Hf 22 Tensile specimens were cut from refractory high entropy alloy ingots and tested for room temperature tensile properties using a universal tensile testing machine. The results are shown in Figure 2. Figure 4 The room temperature tensile elongation of the cast refractory high entropy alloy is 24.1%, indicating that the alloy has good room temperature tensile plasticity.

Claims

1. A method for improving room temperature tensile plasticity of a refractory high entropy alloy, wherein the refractory high entropy alloy is a cast AlCrNbMoTaTiHf alloy. Features: The molar expression of the AlCrNbMoTaTiHf alloy is Al a Cr b Nb c Mo d Ta e Ti f Hf g , where: a = 2 to 8, b = 2 to 6, c = 18 to 28, d = 4 to 9, e = 6 to 14, f = 30 to 40, g ≥ 15, 8 <a+b+d<16,a+b+c+d+e+f+g=100; The preparation process of the AlCrNbMoTaTiHf alloy includes hot isostatic pressing and heat treatment simultaneously, and the process steps are as follows: Step 1: According to the molar expression of the AlCrNbMoTaTiHf alloy, the molar percentage of each component is converted into weight percentage, the metal elements Al, Cr, Nb, Mo, Ta, Ti and Hf are weighed, and the metal raw materials are melted in an electromagnetic suspension melting furnace to obtain a high entropy alloy ingot, and then the alloy ingot is turned over and melted 3 to 6 times and slowly cooled to obtain a cast AlCrNbMoTaTiHf high entropy alloy ingot; Step 2: Place the cast AlCrNbMoTaTiHf high entropy alloy ingot prepared in step 1 in a hot isostatic pressing device, first heat it to 600-800°C, keep it warm for 2-4 hours, then heat it to 1160-1250°C by increasing temperature and pressure, perform hot isostatic pressing at a pressure of not less than 100 MPa, and keep it warm for 1-2 hours; Step 3: Then, the heating is stopped while maintaining the pressure, and the cast AlCrNbMoTaTiHf high entropy alloy ingot is slowly cooled to 1000-1050° C. in the furnace, and then the pressure is released and the ingot is rapidly cooled to room temperature.

2. The method for improving the room temperature tensile plasticity of a refractory high entropy alloy according to claim 1, Features: The raw material purity of the metal elements Al, Cr, Nb, Mo, Ta, Ti and Hf in step 1 is greater than 99.9%.

3. The method for improving room temperature tensile plasticity of a refractory high entropy alloy according to claim 1, Features: The pressure range of the hot isostatic pressing in step 2 is 120-180 MPa.

4. The method for improving room temperature tensile plasticity of a refractory high entropy alloy according to claim 1, Features: The slow cooling rate along with the furnace in step 3 is 60-100° C. / h.

Citation Information

Patent Citations

  • MoxNbTayTiV high-entropy alloy and preparation method thereof

    CN113652593A

  • High-strength refractory high-entropy alloy with low density and excellent tensile plasticity as well as preparation method and application thereof

    CN117165824A

  • Refractory high-entropy alloy material with excellent room-temperature mechanical comprehensive performance and preparation method of refractory high-entropy alloy material

    CN117248147A

  • Preparation method of high-toughness refractory high-entropy alloy

    CN117802436A

  • Method for improving thermal deformation performance of as-cast high-entropy alloy

    CN118345321A