High-performance ferrite free-cutting stainless steel and preparation method thereof

By optimizing the chemical composition and smelting process of stainless steel, combined with high-temperature homogenization treatment and forging process, the problems of brittle fracture and low mechanical properties of existing easy-to-cut stainless steel are solved, and the preparation of high-performance ferrite easy-to-cut stainless steel is achieved. Excellent mechanical properties and good plasticity characteristics.

CN118880200APending Publication Date: 2024-11-01CHONGQING STEEL RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410973370.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing easy-to-cut stainless steels have problems such as brittle fracture, low mechanical properties and poor cutting performance during the smelting process, making it difficult to maintain the good plastic characteristics and mechanical properties of the material.

Method used

The preparation method of high-performance ferrite easy-cut stainless steel is optimized through electric furnace smelting, LF furnace refining, VD furnace degassing treatment and argon protective mold casting technology, and the chemical composition and smelting process of stainless steel are added, and Ca, Ti, V are added. , Nb and other elements form S-Ca-Ti composite easy-to-cut steel, improve grain size and oxidation resistance, and improve the hot and hot plasticity of the material and the finished plasticity through high-temperature homogenization and forging processes.

Benefits of technology

It achieves excellent mechanical properties, elongation and strength of stainless steel, and uniform hardness of forgings, suitable for machining, meeting the needs of high-performance and easy-to-cut stainless steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880200A_ABST
    Figure CN118880200A_ABST
Patent Text Reader

Abstract

The invention discloses high-performance ferrite free-cutting stainless steel, which comprises the following components in percentage by mass: 0.10 to 0.16 percent of C, 0.10 to 0.50 percent of Si, 1.40 to 1.50 percent of Mn, less than or equal to 0.040 percent of P, 0.15 to 0.22 percent of S, 16.00 to 17.50 percent of Cr, 0.30 to 0.50 percent of Mo, 0.001 to 0.006 percent of Ca, 0.015 to 0.10 percent of Ti, 0.08 to 0.24 percent of Nb, 0.08 to 0.24 percent of V, the mass ratio of V + Nb to C is more than or equal to 2, the mass ratio of Mn to S is more than or equal to 6.5, other elements are unavoidable impurities, and the balance of Fe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of free-cutting stainless steel, and in particular to a high-performance ferrite free-cutting stainless steel and a preparation method thereof. Background Art

[0002] In the field of modern equipment manufacturing, with the increasing degree of automation, the processing requirements for precision devices are also getting higher and higher. It is necessary not only to realize automation on the equipment, but also to ensure that the raw materials can meet the requirements of automated processing. In the traditional stainless steel field, problems such as sticking to the tool, difficulty in chip breaking, and large tool wear are prone to occur during the turning process. Therefore, when smelting stainless steel, people add appropriate amounts of free-cutting elements such as sulfur to meet the free-cutting performance, and finally realize the automated production of precision devices. Sulfur will form manganese sulfide (MnS) with manganese in steel. Manganese sulfide in steel can be regarded as a stress concentration source, making the steel easy to cut. Due to the presence of stress concentration sources, the mechanical properties of free-cutting steel are greatly reduced. How to maintain the good plasticity and mechanical properties of steel while ensuring the cutting performance of the material is a difficult problem that needs to be solved urgently in the field of free-cutting steel technology. Summary of the invention

[0003] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a high-performance ferritic free-cutting stainless steel and a preparation method thereof, so as to solve the deficiencies in the existing free-cutting stainless steel production technology, which lead to technical problems such as brittle fracture of the material, low mechanical properties, and poor cutting performance.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] A high-performance ferritic free-cutting stainless steel, which comprises the following components calculated by mass percentage:

[0006] C is 0.10-0.16%, Si is 0.10-0.50%, Mn is 1.40-1.50%, P≤0.040%, S is 0.15-0.22%, Cr is 16.00-17.50%, Mo is 0.30-0.50%, Ca is 0.001-0.006%, Ti is 0.015-0.10%, Nb is 0.08-0.24%, V is 0.08-0.24%, wherein the mass ratio of V+Nb and C is ≥2, the mass ratio of Mn and S is ≥6.5, other elements are unavoidable impurities, and the balance is Fe.

[0007] Preferably, niobium and vanadium have strong affinity with carbon and form corresponding stable compounds with them to refine the structure and grain of steel and change the morphology of sulfides. Nb is 0.08-0.24%, V is 0.08-0.24%, and preferably the mass ratio of V+Nb and C is ≥2, which can fix all carbon in the steel.

[0008] Preferably, in the stainless steel, N, H and O are all harmful elements, and calculated by mass percentage, N≤0.02%, H≤0.0001%, and O≤0.0035%.

[0009] The invention provides a method for preparing high-performance ferritic free-cutting stainless steel, which comprises the following steps: sequentially performing electric furnace smelting, LF furnace refining, VD furnace degassing treatment and argon protection die casting to obtain a stainless steel ingot, and performing high-temperature homogenization treatment, heat processing and heat treatment on the ingot to obtain the stainless steel.

[0010] Preferably, the specific steps of electric furnace smelting are as follows:

[0011] The raw materials are added into the electric arc furnace, and the charge is melted, oxidized, and reduced to remove gas (nitrogen, hydrogen, and oxygen) and inclusions. During the melting period, the oxygen pressure is controlled at 0.5-0.7 kg. During the oxidation period, the oxidation temperature is ≥1570°C, the decarburization amount is controlled to be ≥0.30%, and the high-temperature boiling is ≥10 minutes during the oxidation period; when slag is discharged, the mass percentage of P in the molten steel is controlled to be ≤0.017%, and the molten steel temperature is ≥1650°C. During the reduction period of the electric arc furnace, the composition of the molten steel is adjusted. Calculated by mass percentage, the adjusted molten steel composition meets the following conditions: C: 0.04-0.08%, Si: 0.10-0.30%, Mn: 0.50-1.00%, P: ≤0.017%, Cr: 15.50-16.00%, Mo: 0.28-0.35%; the slag white has good fluidity; when the molten steel temperature is ≥1640°C, it is discharged from the furnace and transferred to the LF furnace.

[0012] Preferably, the specific steps of LF furnace refining are as follows:

[0013] Step 1: The ladle containing molten steel enters the LF furnace station, adjusts the Ar gas flow rate, and measures the temperature; feeds the Al line 0.5-0.8kg / t for strong deoxidation, and the deoxidation products are stirred by blowing argon in the ladle and fully floated and removed. The subsequent addition of chromium and manganese with weak deoxidation ability has a high and stable recovery rate, which is convenient for refining operations.

[0014] Step 2: Add refined slag (calculated by mass percentage, CaO is 55% to 60%, SiO2 is 10% to 15%, Al2O3 is 20% to 30%, and CaF2 is 5% to 10%) to make slag, and add appropriate amounts of C, Si, and Al powder for reduction; the temperature is ≥1570°C, the slag white has good fluidity, and a stable sample is taken for full analysis; the white slag retention time is ≥30min.

[0015] Step 3: According to the analysis results, the composition of the molten steel is adjusted to meet the following conditions, calculated by mass percentage: C: 0.10-0.13%, Si: 0.10-0.30%, Mn: 1.40-1.50%, P: ≤0.030%, Cr: 16.00-17.50%, Mo: 0.30-0.50%; Nb is 0.08-0.24%, V is 0.08-0.24%, wherein the mass ratio of V+Nb and C is ≥2.

[0016] Step 4: When the temperature of the molten steel is 1650-1660°C, fire bricks or quartz sand are added to break up the slag and make acidic slag. The S content is adjusted by adding iron sulfide at a weight percentage of 0.22%.

[0017] Preferably, the VD furnace degassing treatment specifically includes the following steps:

[0018] S1: VD vacuum degree ≤ 67Pa, Ar gas pressure controlled at 0.2-0.4MPa, holding time ≥ 15min;

[0019] S2: Soft blowing after VD for ≥5min, Ar gas pressure is controlled at 0.2-0.4MPa, and the slag surface is not broken;

[0020] S3: Finally, adjust the composition of the molten steel to the controlled composition. Calculated by mass percentage, C is 0.10-0.16%, Si is 0.10-0.50%, Mn is 1.40-1.50%, P≤0.040%, S is 0.15-0.22%, Cr is 16.00-17.50%, Mo is 0.30-0.50%, Ca is 0.001-0.006%, Ti is 0.015-0.10%, Nb is 0.08-0.24%, and V is 0.08-0.24%, wherein the mass ratio of V+Nb and C is ≥2, and the mass ratio of Mn / S is ≥6.5;

[0021] After the chemical composition of the molten steel is adjusted to meet the requirements, the pouring temperature is 1540-1550℃.

[0022] Preferably, the specific steps of the argon protection die casting are as follows:

[0023] Step 1: Clean the inner wall of the ingot mold to prevent carbon increase or subcutaneous pores; the ladle calming time is 5-8 minutes; the amount of protective slag is 1.5-2.0kg / t, and the amount of exothermic agent is 0.5-1.0kg / t.

[0024] Step 2: The pouring temperature of the steel ingot is 1540-1550℃; Ar gas protection is carried out throughout the pouring process, and the distance between the water inlet and the fiber argon curtain ring is shortened as much as possible. After the riser is installed, the flow is appropriately reduced to ensure good riser shrinkage compensation.

[0025] Preferably, the specific steps of the high temperature homogenization treatment are as follows:

[0026] Step 1: The temperature of the heating furnace must be ≤500℃ before the steel ingot can enter the furnace.

[0027] Step 2: The heating rate of the heating furnace is ≤100℃ / hour, and the temperature is kept at 900℃ for 3 hours, and then the temperature is continued to rise (the heating rate is controlled at ≤100℃ / hour).

[0028] Step 3: Heat the furnace to 1260-1280°C, and keep warm for ≥16h.

[0029] Step 4: Cool the furnace to 500°C and air cool after removing from the furnace.

[0030] Preferably, the specific steps of the thermal processing are as follows:

[0031] Among them, the forging adopts the direct drawing process, appropriately increasing the forging ratio of the ingot to ensure that the minimum forging ratio reaches above 8.

[0032] Step 1: The starting forging temperature of the steel ingot is 1120-1160°C, and the final forging temperature is ≥850°C;

[0033] Step 2: Forging the intermediate blank obtained in step 1 into a forging blank (double size); wherein the start forging temperature is 1100-1120° C., the last fire forging pressure ratio is 1.5-2.0; and the final forging temperature is ≥850° C.;

[0034] Preferably, the heat treatment is to heat treat the forging blank obtained in step 2, and the heat treatment method is quenching and tempering; the specific steps are as follows:

[0035] S1: Forgings need to be stacked flat when entering the furnace, and the horizontal and vertical spacing between each forging needs to be ≥40mm.

[0036] S2: The quenching process of forgings is: holding temperature 1040-1060℃, holding time 1-1.5h, and immediate water cooling;

[0037] S3: The process parameters for tempering the forgings after S2 quenching are as follows: holding temperature 680-720°C, holding time 3-5 hours, and hanging out for air cooling.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] 1. The present invention optimizes the chemical composition of stainless steel, forms S-Ca-Ti composite free-cutting steel by adding Ca and Ti free-cutting elements, improves the cutting performance of forgings, and improves the oxidation resistance of ferrite free-cutting stainless steel; adds V+Nb alloy to increase the grain size of steel and improve the morphology of sulfides.

[0040] 2. The present invention also adjusts the smelting process of stainless steel, adopts the new high-purity process technology of "electric furnace + LF + VD + die casting" for easy-to-cut stainless steel, reduces the content of hydrogen, oxygen and nitrogen in steel, reduces the hard points of high-hardness compounds in steel, and improves the cold and hot plasticity of materials and the plasticity of finished products. The steel ingot is treated with high-temperature homogenization, and the forging process adopts the direct drawing process. The forging ratio of the steel ingot is appropriately increased to ensure that the minimum forging ratio reaches more than 8. After the intermediate billet is repaired, the last fire forging ratio = 1.5-2.0, and the forging is forged into the forging blank specification. The sulfide inclusions in the steel exist in the form of spindles and dot balls, which retains the plastic characteristics of the steel and makes it have better elongation and tensile properties.

[0041] 3. The high-performance ferritic free-cutting stainless steel prepared by the present invention has achieved the expected design goals in terms of chemical composition, macrostructure, metallographic structure, morphology and distribution characteristics of manganese sulfide, mechanical properties, and ultrasonic flaw detection of the finished forgings, which can fully meet the needs, have excellent mechanical properties, and significantly improved elongation and strength. The hardness of the forgings is uniform and consistent, which is convenient for subsequent machining. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The following are low-magnification organization diagrams of Example 1 and the comparative example; wherein a is the comparative example and b is Example 1.

[0043] Figure 2 This is a comparative grain size detection diagram; a is the horizontal direction and b is the vertical direction.

[0044] Figure 3 The morphology and distribution characteristics of manganese sulfide in Example 1 and the comparative example forgings; wherein a is the comparative example and b is Example 1.

[0045] Figure 4 This is the stacking layout diagram of the forgings heat treatment in Example 1. DETAILED DESCRIPTION

[0046] The present invention will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the present invention belong to the scope of protection of the present invention.

[0047] Unless otherwise indicated in specific cases in the present invention, the numerical ranges listed herein include the upper and lower limits, and all integers and fractions within the range, and are not limited to the specific values ​​listed when defining the range.

[0048] 1. A high-performance ferritic free-cutting stainless steel

[0049] Calculated by mass percentage, the stainless steel includes the following components:

[0050] C is 0.10-0.16%, Si is 0.10-0.50%, Mn is 1.40-1.50%, P≤0.040%, S is 0.15-0.22%, Cr is 16.00-17.50%, Mo is 0.30-0.50%, Ca is 0.001-0.006%, Ti is 0.015-0.10%, Nb is 0.08-0.24%, V is 0.08-0.24%, wherein the mass ratio of V+Nb and C is ≥2, the mass ratio of Mn and S is ≥6.5, other elements are unavoidable impurities, and the balance is Fe.

[0051] In the prior art, sulfur is often added to improve the cutting performance of stainless steel. For example, y1Cr17Mo is a sulfur-containing free-cutting steel. In y1Cr17Mo stainless steel, sulfur forms MnS inclusions with manganese in the steel, interrupting the continuity of the base metal, causing undercutting when the steel is deformed at high speed during cutting, breaking the chips through stress concentration, and achieving the purpose of improving the cutting performance of the steel. Therefore, in this type of free-cutting steel, sulfur is added as a beneficial element to improve the cutting performance of the steel. However, sulfur is easy to segregate in steel, deteriorating the quality of steel, and reducing the plasticity of steel at high temperatures. From this point of view, it is also a harmful element. It exists in the form of FeS with a lower melting point. The melting point of FeS alone is only 1190°C, and the eutectic temperature of FeS in steel is even lower, only 988°C. When the steel solidifies, iron sulfide precipitates at the primary grain boundaries. When steel is hot-worked at 1100-1200℃, FeS on the grain boundary will melt, greatly weakening the bonding force between the grains, leading to hot brittleness of the steel. In addition, due to the presence of stress concentration sources, the mechanical properties of the steel will eventually be reduced.

[0052] In order to solve the above technical problems, the present invention considers improving the cutting steel from two aspects. First, from the component aspect, in order to prevent the brittleness of y1Cr17Mo caused by high sulfur, by ensuring that the free-cutting steel contains enough manganese, it forms MnS inclusions with a higher melting point. And the mass content ratio of Mn and S in the steel is preferably ≥5, more preferably 5-8, and most preferably 6-7. By adding Ca and Ti free-cutting elements, S-Ca-Ti composite free-cutting steel is formed to improve the cutting performance of forgings; adding V and Nb alloy elements increases the grain size of the steel and improves the morphology of sulfides. Secondly, from the process route, the new high-purity process technology route of "electric furnace + LF + VD + die casting" is adopted to reduce the hydrogen, oxygen and nitrogen gas content in the steel, reduce the hard points of high-hardness compounds in the steel, and improve the cold and hot plasticity of the material and the plasticity of the finished product; the steel ingot is treated with high-temperature homogenization, and the forging adopts the direct drawing process, and the forging ratio of the steel ingot is appropriately increased to ensure that the minimum forging ratio reaches more than 8, and the last fire forging ratio = 1.5~2.0), and the sulfide inclusions in the steel exist in the form of spindles and dot balls, which ensures the plastic characteristics of the steel and makes it have good tensile properties; when quenching and tempering, the forgings need to be hoisted and stacked flat, and stacked in one layer. The horizontal and vertical spacing between each forging needs to be ≥40mm to ensure that the temperature of the forgings is uniform during heat treatment, so that the hardness of the forgings is uniform. The high-performance ferrite easy-to-cut stainless steel forgings produced have excellent mechanical properties, obvious strength improvement, uniform hardness, and are convenient for subsequent machining.

[0053] In some embodiments, the present invention controls the C content appropriately. When the carbon content is too low, a large amount of ferrite will appear, the hardness will be reduced, and it will easily stick to the blade during cutting, and the surface of the processed material will be rough. When the carbon content is too high, the hardness will also increase, the cutting resistance will increase, the cutting performance will deteriorate, and the corrosion resistance of the material will decrease. Therefore, calculated by mass percentage, the C content is controlled at 0.10-0.16%, preferably 0.11-0.13%, and can be 0.1%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, etc., as well as all ranges and sub-ranges between the above values.

[0054] In some embodiments, silicon (Si) has a harmful effect on the machinability of stainless steel. Silicon is dissolved in ferrite, which increases the hardness of steel and makes cutting difficult; silicon combines with oxygen in steel to form silicon oxide inclusions with higher hardness, which increases tool wear and reduces service life; silicon also reduces the oxygen content in stainless steel, deteriorating the machinability of steel. Therefore, calculated by mass percentage, the Si content is controlled at 0.10-0.50%, preferably 0.15-0.25%, and can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, etc., as well as all ranges and sub-ranges between the above values.

[0055] In some embodiments, manganese (Mn) and sulfur form manganese sulfide inclusions, which make the chips easy to break and improve the machinability of the steel; the hot brittleness caused by sulfur can be eliminated or weakened. In order to prevent the brittleness caused by sulfur, it is usually ensured that the free-cutting steel contains enough manganese to form MnS inclusions with a higher melting point, and the mass content ratio of Mn to S in the steel is preferably ≥5, more preferably 5-8, and most preferably 6-7.

[0056] In some embodiments, the present invention adds Ti to steel, and titanium is the composite free-cutting additive of the present invention, which reduces the bonding wear of the tool, reduces chip accumulation, and improves the surface roughness of the workpiece; increases the amount of austenite of ferritic stainless steel at high temperature, prevents coarse grains, and refines the grains; and can also improve the oxidation resistance of ferritic free-cutting stainless steel. Therefore, calculated by mass percentage, the addition amount of Ti is 0.015-0.10%, preferably 0.03-0.05%, and can be 0.015%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, etc., as well as all ranges and sub-ranges between the above values.

[0057] In some embodiments, Ca is added to the stainless steel. Calcium is a composite free-cutting additive of the present invention. Calcium can improve the morphology of sulfides to make them spheroidized and large-scale. Ca and Ti, S and other free-cutting elements form S-Ca-Ti composite free-cutting steel, which improves the cutting performance of forgings and the oxidation resistance of ferrite free-cutting stainless steel. Therefore, the content of Ca is controlled between 0.001 and 0.006%, preferably 0.001 to 0.003%, and can be 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, etc., as well as all ranges and sub-ranges between the above values.

[0058] In some embodiments, 0.08-0.24% Nb and 0.08-0.24% V are added simultaneously. Preferably, the mass ratio of V+Nb to C is ≥2, which can fix all carbon in the steel, increase the grain size of the steel, and improve the morphology of sulfides.

[0059] In some embodiments, in the stainless steel, N, H and O are harmful elements, and calculated by mass percentage, N≤0.02%, H≤0.0001%, and O≤0.0035%.

[0060] 2. A method for preparing high-performance ferritic free-cutting stainless steel

[0061] The method of the present invention adopts a new high-purity process technology route of "electric furnace + LF + VD + die casting" to obtain the steel ingot of the free-cutting stainless steel.

[0062] In some embodiments, to ensure the purity of the smelting process, the raw materials of the electric furnace use the same steel grade that has been refined and degassed to return scrap steel and molten iron to prevent the introduction of too many residual elements from the source. The electric furnace primary smelting is reasonable in oxygen blowing, reasonable decarburization, and reasonable slag making, and the molten steel boils evenly to achieve the purpose of degassing and removing inclusions; the steel and slag retention operations are adopted to prevent the oxide slag from entering the refining bag. The specific steps of the electric furnace smelting are as follows:

[0063] The raw materials are added into the electric arc furnace for melting, oxidation and reduction smelting to remove gases (nitrogen, hydrogen and oxygen) and inclusions. The oxygen pressure is controlled at 0.5-0.7kg during the melting period. During the oxidation period, the oxidation temperature is ≥1570℃, the decarburization amount is controlled to be ≥0.30%, and the high temperature boiling is ≥10min during the oxidation period; when slag is discharged, the mass percentage of P in the molten steel is controlled to be ≤0.017%, and the molten steel temperature is ≥1650℃. During the reduction period of the electric arc furnace, the composition of the molten steel is adjusted to meet the following conditions. Calculated by mass percentage, the adjusted molten steel composition is: C: 0.04-0.08%, Si: 0.10-0.30%, Mn: 0.50-1.00%, P: ≤0.017%, Cr: 15.50-16.00%, Mo: 0.28-0.35%; the slag has good fluidity; when the molten steel temperature is ≥1640℃, it is taken out of the furnace and transferred to the LF furnace.

[0064] In some embodiments, the LF furnace refines the white slag in the ladle barrel by blowing argon into the ladle barrel for stirring in a low-oxygen (oxygen content <5%) atmosphere and heating the molten steel that has passed through the primary refining furnace with a graphite electrode. Since argon stirring accelerates the chemical reaction between slag and steel, temperature compensation by arc heating can ensure a longer refining time, thereby reducing the content of oxygen, sulfur and inclusions in the steel. Argon blowing is the driving force for the flow of molten steel in the LF furnace ladle, and good bottom argon blowing conditions are the key to the floating of deoxidized inclusions in steel. During the LF furnace refining process, an Ar blowing mode of large gas volume first and small gas volume later is adopted. After the large gas volume is blown, the gas volume is reduced to 40% to 50% for 5 to 10 minutes of small gas volume treatment, which is conducive to the removal of inclusions. The refined slag of the LF furnace is required to have a low melting point, suitable viscosity, surface tension and refined slag composition. By reasonably controlling the type and amount of the slag used, the reducibility of the slag is maintained, and the molten steel [Al], [O], [Ca], [Mg], etc. are controlled through the slag-steel reaction, and then the inclusions are stably controlled through the molten steel [Al], [O], [Ca], [Mg], etc., to meet the purposes of desulfurization, deoxidation, control of inclusion morphology, adsorption of inclusions in steel, formation of foam slag, guarantee of submerged arc effect, and improvement of thermal efficiency. The production of the LF furnace uses a special refined slag, which includes the following components calculated by mass percentage: CaO 55% to 60%, SiO2 10% to 15%, Al2O3 20% to 30%, CaF2 5% to 10%. The LF white slag is kept for ≥30 minutes, and the composition of the molten steel is adjusted to the controlled composition according to the analysis results. When the temperature is appropriate, fire bricks or quartz sand are added to break the slag. S is adjusted to a mass percentage of 0.22% by adding iron sulfide.

[0065] The specific steps of LF furnace refining are as follows:

[0066] The ladle containing molten steel enters the LF furnace station, adjusts the Ar gas flow rate, and measures the temperature; feeds Al wire 0.5-0.8kg / t for strong deoxidation, and the deoxidation products are stirred by argon blowing in the ladle and fully floated and removed. The subsequent addition of chromium and manganese with weak deoxidation ability has a high and stable recovery rate, which brings convenience to refining. Add refined slag (calculated by mass percentage, the refined slag contains the following components: CaO 55%-60%, SiO2 10%-15%, Al2O3 20%-30%, CaF2 5%-10%) to make slag, add appropriate amounts of C, Si, and Al powder for reduction; the temperature is ≥1570°C, the slag white has good fluidity, and a stable sample is taken for full analysis; the white slag retention time is ≥30min, and the composition of the molten steel is adjusted according to the analysis results to meet the following conditions, by mass percentage: C: 0.10-0.13%, Si: 0.10-0.30%, Mn: 1.40-1.50%, P: ≤0.030%, Cr: 16.00-17.50%, Mo: 0.30-0.50%; Nb is 0.08-0.24%, V is 0.08-0.24%, and the mass ratio of V+Nb and C is ≥2. The temperature of the molten steel is 1650-1660℃, fire bricks or quartz sand are added to break up the slag and make acidic slag. The S content is adjusted by adding iron sulfide at a mass percentage of 0.22%.

[0067] In some embodiments, the molten steel after LF furnace refining is placed in a vacuum tank (vacuum chamber) and subjected to bottom blowing argon stirring and vacuum degassing process, which has good degassing and deoxidation effects, can effectively reduce the hydrogen and nitrogen content in the steel, remove oxygen in the steel through carbon-oxygen reaction, and also has the function of uniform composition and temperature to obtain pure molten steel. The VD furnace degassing treatment specifically includes the following steps:

[0068] S1: VD vacuum degree ≤ 67Pa, Ar gas pressure controlled at 0.2-0.4MPa, holding time ≥ 15min;

[0069] S2: Soft blowing after VD for ≥5min, Ar pressure is controlled at 0.2-0.4MPa, and the slag surface is not blown; from the completion of VD vacuum to before pouring, the molten steel and slag are covered during the whole process to prevent the molten steel from contacting and inhaling air.

[0070] S3: Adjust the composition of the molten steel to meet the following conditions:

[0071] Finally, the composition of the molten steel is adjusted to meet the following conditions: calculated by mass percentage, C is 0.10-0.16%, Si is 0.10-0.50%, Mn is 1.40-1.50%, P≤0.040%, S is 0.15-0.22%, Cr is 16.00-17.50%, Mo is 0.3-0.50%, Ca is 0.001-0.006%, Ti is 0.015-0.10%, Nb is 0.08-0.24%, V is 0.08-0.24%, wherein the mass ratio of V+Nb and C is ≥2, and the mass ratio of Mn / S is ≥6.5;

[0072] After the chemical composition of the molten steel is adjusted, the pouring temperature is 1540-1550℃.

[0073] In some embodiments, the specific steps of casting the steel ingot are as follows:

[0074] Step 1: Clean the inner wall of the ingot mold to prevent carbon increase or subcutaneous pores; the ladle calming time is 5-8 minutes; the amount of protective slag is 1.5-2.0kg / t, and the amount of exothermic agent is 0.5-1.0kg / t.

[0075] Step 2: The pouring temperature of the steel ingot is 1540-1550℃; Ar gas protection is carried out throughout the pouring process, and the distance between the water inlet and the fiber argon curtain ring is shortened as much as possible. After the riser is installed, the flow is appropriately reduced to ensure good riser shrinkage compensation.

[0076] In some embodiments, the specific steps of the high temperature homogenization treatment of the steel ingot are as follows:

[0077] Step 1: The temperature of the heating furnace must be ≤500℃ before the steel ingot can enter the furnace.

[0078] Step 2: The heating rate of the heating furnace is ≤100℃ / hour. Keep the temperature at 900℃ for 3 hours and then continue to heat up (heating rate ≤100℃ / hour).

[0079] Step 3: Heat the furnace to 1260-1280°C, and keep warm for ≥16h.

[0080] Step 4: Cool the furnace to 500°C and air cool after removing from the furnace.

[0081] In some embodiments, the specific steps of the steel ingot forging hot working are as follows:

[0082] Among them, the forging adopts the direct drawing process, appropriately increasing the forging ratio of the ingot to ensure that the minimum forging ratio reaches above 8.

[0083] Step 1: The starting forging temperature of the steel ingot is 1120-1160°C, and the final forging temperature is ≥850°C;

[0084] Step 2: Forging the intermediate blank obtained in step 1 into a forging blank (double size); wherein the start forging temperature is 1100-1120° C., the last fire forging pressure ratio is 1.5-2.0; and the final forging temperature is ≥850° C.;

[0085] In some embodiments, the specific steps of heat treating the forging blank are as follows:

[0086] Among them, the heat treatment methods are quenching and tempering;

[0087] S1: Forgings need to be stacked flat when entering the furnace, and the horizontal and vertical spacing between each forging needs to be ≥40mm.

[0088] S2: The quenching process of forgings is: holding temperature 1040-1060℃, holding time 1-1.5h, and immediate water cooling;

[0089] S3: The process parameters for tempering the forgings after S2 quenching are as follows: holding temperature 680-720°C, holding time 3-5 hours, and hanging out for air cooling.

[0090] 3. Examples and Comparative Examples

[0091] Example 1

[0092] (1) Electric arc furnace smelting

[0093] The raw materials are added into the electric arc furnace, and the charge is melted, oxidized, and reduced to remove gas (nitrogen, hydrogen, and oxygen) and inclusions. During the melting period, the oxygen pressure is controlled at 0.5-0.7 kg. During the oxidation period, the oxidation temperature is ≥1570°C, the decarburization amount is controlled to be ≥0.30%, and the high-temperature boiling is ≥10 minutes during the oxidation period; when slag is discharged, the mass percentage of P in the molten steel is controlled to be ≤0.017%, and the molten steel temperature is ≥1650°C. During the reduction period of the electric arc furnace, the composition of the molten steel is adjusted according to the mass percentage: C: 0.04-0.08%, Si: 0.10-0.30%, Mn: 0.50-1.00%, P: ≤0.017%, Cr: 15.50-16.00%, Mo: 0.28-0.35%; the slag white has good fluidity; when the molten steel temperature is ≥1640°C, it is discharged from the furnace and transferred to the LF furnace.

[0094] (2) LF refining:

[0095] The ladle containing molten steel enters the LF furnace station, adjusts the Ar gas flow rate, and measures the temperature; feeds the Al line 0.5-0.8kg / t for strong deoxidation, and the deoxidation products are stirred by blowing argon in the ladle and fully floated and removed. The subsequent addition of chromium and manganese with weak deoxidation ability has a high and stable recovery rate, which is convenient for refining operations.

[0096] Refining slag (CaO 55% ~ 60%, SiO2 10% ~ 15%, Al2O3 20% ~ 30%, CaF2 5% ~ 10%) is used to make slag, and appropriate amount of C, Si, Al powder is added for reduction; the temperature is ≥ 1570℃, the slag white has good fluidity, and a stable sample is taken for full analysis; the white slag retention time is ≥ 30min.

[0097] According to the analysis results, the composition of the molten steel is adjusted to the controlled composition, according to the mass percentage: C: 0.10-0.13%, Si: 0.10-0.30%, Mn: 1.40-1.50%, P: ≤0.030%, Cr: 16.00-17.50%, Mo: 0.30-0.50%; Nb is 0.08-0.24%, V is 0.08-0.24%, among which the mass ratio of V+Nb and C is ≥2.

[0098] The temperature of the molten steel is 1650-1660℃, fire bricks and quartz sand are added to break up the slag and make acidic slag. The S content is adjusted by adding iron sulfide at a weight percentage of 0.22%.

[0099] (3) VD vacuum degree ≤ 67Pa, Ar gas 0.2-0.4MPa, holding time ≥ 15min.

[0100] (4) Soft blowing after VD for ≥5min, Ar gas 0.2-0.4MPa, can not blow the slag surface. Finally, adjust the composition of molten steel to the control composition, according to mass percentage:

[0101] C is 0.10-0.16%, Si is 0.10-0.50%, Mn is 1.40-1.50%, P≤0.040%, S is 0.15-0.22%, Cr is 16.00-17.50%, Mo is 0.3-0.50%, Ca is 0.001-0.006%, Ti is 0.015-0.10%, Nb is 0.08-0.24%, V is 0.08-0.24%, wherein the mass ratio of V+Nb and C is ≥2, and the mass ratio of Mn / S is ≥6.5;

[0102] Temperature for pouring out of the tank: 1540-1550℃.

[0103] (5) Casting: Ingot mold 1.7t. Clean the inner wall of the ingot mold to prevent carbon increase or subcutaneous pores. Ladle calming time 5-8min. Protective slag 1.5-2.0kg / t, exothermic agent 0.5-1.0kg / t.

[0104] (6) High temperature homogenization treatment of steel ingots: temperature 1260-1280℃, insulation ≥16h.

[0105] (7) Forging (forging ratio ≥ 6): The starting forging temperature of the steel ingot is 1160°C, and the ingot is drawn into a 200×200×L square billet. The final forging temperature is ≥850°C and slowly cooled.

[0106] (8) Forging into forging blank (forging ratio ≥ 2): the opening forging temperature of the intermediate blank is 1120℃, the forged forging blank specification is 128*130*440mm (fixed length), the last fire forging ratio is ≥1.5-2.0; the final forging temperature is ≥850℃.

[0107] (9) Heat treatment of forgings: Heat treatment method: quenching + tempering

[0108] Quenching: Holding temperature 1040 ~ 1060 ℃, holding time 1 ~ 1.5 hours, immediately take out of the furnace and water cool.

[0109] Tempering: holding temperature 680 ~ 720 ℃, holding time 3 ~ 5 hours, air cooling.

[0110] During quenching and tempering, the forgings need to be hoisted and stacked neatly in the furnace, one layer at a time, and the horizontal and vertical spacing between each forging needs to be ≥40mm (see the attached diagram for the stacking layout of forgings for heat treatment). Figure 4 ).

[0111] The same method as in Example 1 was adopted to prepare Examples 2 to 3 meeting the component requirements of Table 1; meanwhile, y1Cr17Mo steel prepared by conventional smelting method was used as a comparative example to be compared with the examples of the present invention.

[0112] Table 1 (Unit: wt%)

[0113]

[0114] Note: "--" in Table 1 means that there is no requirement in the standard for y1Cr17Mo steel (comparative example), and alloy elements are not actively added.

[0115] 4. Performance Comparison

[0116] 1. Low-magnification tissue

[0117] The stainless steel prepared in the example was subjected to a macroscopic inspection according to the standard GB / T226-2015. The macroscopic structure and inspection results are shown below: Figure 1 And Table 2 below.

[0118] Table 2 Low-power test results of examples and comparative examples (unit: level)

[0119] Compare Projects Generally loose Loose center Segregation Example 1 0.5 0.5 0.5 Example 2 0.5 0.5 0.5 Example 3 0.5 0.5 0.5 Comparative Example 0.5 0.5 1.5

[0120] Figure 1 In the example, a is a comparative example, b is Example 1, Figure 1It can be seen that the overall acid etching degree of the macroscopic sample of Example 1 is uniform, no corrosion pits appear, and no defects such as bubbles, shrinkage cavities, cracks, slag inclusions, etc.; the evaluation of general looseness, central looseness, and segregation of the macroscopic structure are all 0.5 level.

[0121] The overall acid etching degree of the low-magnification specimens of the comparative example is uniform, without corrosion pits, bubbles, shrinkage cavities, cracks, slag inclusions and other defects; the general looseness and central looseness of the low-magnification structure are both level 0.5, and the segregation evaluation is level 1.5, indicating that the distribution of alloy elements in the material of the comparative sample is obviously uneven, which will lead to uneven mechanical properties of the comparative material. This unevenness leads to quality problems such as breakage or failure of the steel during use.

[0122] After the process is improved, the embodiment is more uniform than the comparative example and the segregation of the forging is reduced.

[0123] 2. Metallographic structure

[0124] The grain size is tested according to the standard GB / T6394-2017. After the forging blank is tempered, a sample is cut at the 1 / 4 position of the remaining blank. After the surface is ground and polished, it is etched with a 4% nitric acid alcohol solution. Figure a is horizontal, showing white carbide particles along the grain boundaries and in the crystals. The oval gray in the figure is sulfide, and there is no abnormal structure. Figure b is vertical, showing a large number of gray long strips of sulfide, without abnormal structure. The horizontal and vertical samples of the embodiment have no abnormal structure, and the grain size is level 7, which is fine-grained steel. As the grain size is refined and reduced, the strength and plasticity of the material are improved.

[0125] 3. Morphology and distribution characteristics of manganese sulfide

[0126] According to GB 10561, the non-metallic inclusions are detected. The polished surface parallel to the longitudinal axis (longitudinal surface) of the steel is about 200 square millimeters (20mm×10mm). Observe under a metallographic microscope. The square field of view (such as Figure 3 (shown)

[0127] Before process improvement ( Figure 3 a), in the y1Cr17Mo steel prepared by the prior art, the sulfide is in the shape of long strips, with a length of generally 100 to 200 μm and an aspect ratio of 5 to 10. After the process is improved ( Figure 3 b) In the stainless steel prepared in Example 1, the sulfides are discontinuous and dot-shaped, with a length of 5 to 30 μm and an aspect ratio of 2 to 5. The sulfides are smaller in size and have a smaller aspect ratio.

[0128] In the comparative example obtained by the traditional smelting method before the process improvement, the elongated strip-shaped sulfides destroyed the continuity of the steel matrix and accelerated the brittle fracture of the transverse tensile. In the smelting method of Example 1, the sulfides were dispersed in a discontinuous and dot-spherical shape, which retained the plastic characteristics of the steel, and the elongation was greatly increased, so that it had better transverse tensile properties.

[0129] 4. Mechanical properties

[0130] The mechanical properties of the embodiments and comparative examples were tested, and the results are shown in Table 3.

[0131] Table 3

[0132]

[0133] According to the technical conditions of standard steel forgings, samples were taken from the forgings after heat treatment, and the results of mechanical property testing were (see Table 3). Compared with the comparative example, the tensile strength of the embodiment increased by 127MPa, the elongation increased by 6.33%, and the cross-sectional shrinkage increased by 6.67%. The mechanical properties of the stainless steel prepared in the embodiment increased by 16.89%, which is quite obvious; the plastic characteristics (elongation) increased by 29.01%, which is a significant increase, so that it has better transverse tensile properties.

[0134] From the above test results, it can be seen that the high-performance ferrite free-cutting stainless steel prepared by the present invention and the finished forging product inspection indicators fully meet the customer's technical agreement and relevant standard requirements, with excellent mechanical properties and significantly improved plasticity characteristics (elongation).

[0135] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.

Claims

1. A high-performance ferritic free-cutting stainless steel, characterized in that: Calculated by mass percentage, the stainless steel includes the following components: C is 0.10-0.16%, Si is 0.10-0.50%, Mn is 1.40-1.50%, P≤0.040%, S is 0.15-0.22%, Cr is 16.00-17.50%, Mo is 0.30-0.50%, Ca is 0.001-0.006%, Ti is 0.015-0.10%, Nb is 0.08-0.24%, V is 0.08-0.24%, wherein the mass ratio of V+Nb and C is ≥2, the mass ratio of Mn and S is ≥6.5, other elements are unavoidable impurities, and the balance is Fe.

2. The stainless steel according to claim 1, characterized in that: Calculated by mass percentage, in the stainless steel, Nb is 0.08-0.24%, V is 0.08-0.24%, and the mass ratio of V+Nb to C is ≥2.

3. The stainless steel according to claim 1, characterized in that: In the stainless steel, N, H and O are all harmful elements. Calculated by mass percentage, N≤0.02%, H≤0.0001%, and O≤0.0035%.

4. A method for preparing high-performance ferritic free-cutting stainless steel, characterized in that: The stainless steel ingot is obtained after electric furnace smelting, LF furnace refining, VD furnace degassing and argon protection mold casting, and then the ingot is subjected to high-temperature homogenization treatment, heat processing and heat treatment in sequence to obtain the stainless steel.

5. The preparation method according to claim 4, characterized in that: The specific steps of electric furnace smelting are as follows: Step 1: Add raw materials into an electric arc furnace, melt, oxidize and reduce the materials to remove gas and inclusions; during the melting period, the oxygen pressure is controlled at 0.5-0.7 kg; Step 2: During the oxidation period, the oxidation temperature is ≥1570°C, the decarburization amount is controlled to be ≥0.30%, and the high-temperature boiling is ≥10min during the oxidation period; when slag is discharged, the mass percentage of P in the molten steel is controlled to be ≤0.017%, and the molten steel temperature is ≥1650°C; Step 3: During the arc furnace reduction period, adjust the composition of the molten steel. Calculate by mass percentage. The adjusted molten steel composition meets the following conditions: C: 0.04~0.08%, Si: 0.10~0.30%, Mn: 0.50~1.00%, P: ≤0.017%, Cr: 15.50~16.00%, Mo: 0.28~0.35%; Step 4: When the slag has good fluidity and the molten steel temperature is ≥1640℃, it is taken out of the furnace and transferred to LF furnace.

6. The preparation method according to claim 5, characterized in that: The specific steps of LF furnace refining are as follows: Step 1: The ladle containing molten steel enters the LF furnace station, adjusts the Ar gas flow rate, and measures the temperature; feeds 0.5-0.8 kg / t of Al wire for strong deoxidation, and the deoxidation products are stirred by blowing argon in the ladle and fully floated and removed; Step 2: Add refined slag for slagging, add C, Si, Al powder for reduction; temperature ≥1570℃, slag white fluidity is good, take stable sample for full analysis; white slag retention time ≥30min; Step 3: According to the analysis results, the composition of the molten steel is adjusted to meet the following conditions: calculated by mass percentage: C: 0.10-0.13%, Si: 0.10-0.30%, Mn: 1.40-1.50%, P: ≤0.030%, Cr: 16.00-17.50%, Mo: 0.30-0.50%; Nb is 0.08-0.24%, V is 0.08-0.24%, wherein the mass ratio of V+Nb to C is ≥2; Step 4: When the temperature of the molten steel is 1650-1660°C, fire bricks or quartz sand are added to break up the slag and make acidic slag; S is adjusted by adding iron sulfide at a mass percentage of 0.22%.

7. The preparation method according to claim 5, characterized in that: The VD furnace degassing process specifically includes the following steps: S1: VD vacuum degree ≤ 67Pa, Ar gas pressure controlled at 0.2-0.4MPa, holding time ≥ 15min; S2: Soft blowing after VD for ≥5min, Ar gas pressure is controlled at 0.2-0.4MPa, and the slag surface is not broken; S3: Adjust the composition of the molten steel to meet the following conditions: Calculated by mass percentage, C is 0.10-0.16%, Si is 0.10-0.50%, Mn is 1.40-1.50%, P≤0.040%, S is 0.15-0.22%, Cr is 16.00-17.50%, Mo is 0.30-0.50%, Ca is 0.001-0.006%, Ti is 0.015-0.10%, Nb is 0.08-0.24%, V is 0.08-0.24%, wherein the mass ratio of V+Nb and C is ≥2, and the mass ratio of Mn / S is ≥6.5; After the chemical composition of the molten steel is adjusted to meet the requirements, the pouring temperature is 1540-1550℃.

8. The preparation method according to claim 5, characterized in that: The specific steps of the argon protection die casting are as follows: Step 1: Clean the inner wall of the ingot mold; the ladle calming time is 5-8min; the amount of protective slag is 1.5-2.0kg / t, and the amount of exothermic agent is 0.5-1.0kg / t; Step 2: The pouring temperature of the steel ingot is 1540-1550°C; Ar gas protection is carried out throughout the pouring process.

9. The preparation method according to claim 8, characterized in that: The specific steps of the high temperature homogenization treatment are as follows: Step 1: The furnace temperature of the heating furnace is ≤500℃, and the steel ingot is put into the furnace; Step 2: The heating furnace is heated at a rate of ≤100°C / hour, and the temperature is kept at 900°C for 3 hours, and then the temperature is continued to be raised and the heating rate is controlled to be ≤100°C / hour; Step 3: Heat the furnace to 1260-1280°C, and keep warm for ≥16h; Step 4: Cool the furnace to 500°C and air cool after removing from the furnace.

10. The preparation method according to claim 9, characterized in that: The thermal processing comprises the following steps: Step 1: The starting forging temperature of the steel ingot is 1120-1160°C, and the final forging temperature is ≥850°C; Step 2: Forging the intermediate blank obtained in step 1 into a forging blank; wherein the start forging temperature is 1100-1120°C, the last fire forging pressure ratio is 1.5-2.0; and the final forging temperature is ≥850°C; The heat treatment is to heat treat the forging blank obtained in step 2, and the heat treatment method is quenching and tempering, and the specific steps are as follows: S1: Forgings need to be stacked flat when entering the furnace, and the horizontal and vertical spacing between each forging should be ≥40mm; S2: The quenching process of forgings is: holding temperature 1040-1060℃, holding time 1-1.5h, and immediate water cooling; S3: The process parameters for tempering the forgings after S2 quenching are as follows: holding temperature 680-720°C, holding time 3-5 hours, and hanging out for air cooling.