Manufacturing method of amorphous motor iron core
By finely controlling the raw material ratio and process of amorphous alloys, and optimizing the molding and heat treatment processes, the problem of insufficient performance of traditional motor core materials is solved, and high-efficiency and low-loss amorphous motor core manufacturing is achieved, improving magnetism and machinery Performance, meet the energy-saving and environmental protection needs of modern motors.
Patent Information
- Application Number
- CN202410934605.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-01
AI Technical Summary
The magnetic properties of traditional motor core materials are insufficient, have large losses and are heavy in weight, which cannot meet the efficient, energy-saving and environmentally friendly needs of modern motors.
By finely controlling the raw material ratio, optimized molding and heat treatment processes of amorphous alloys, including smelting, rapid cooling, crushing, pre-pressing, fine pressing, annealing, crystallization treatment, magnetic field treatment and surface strengthening treatment, we produce high efficiency and low efficiency Lossed amorphous motor core.
It realizes efficient and low-loss manufacturing of amorphous motor core, improves magnetic and mechanical properties, reduces energy consumption, and meets the energy-saving and environmental protection requirements of modern motors.
Smart Images

Figure CN118880201A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron cores, and in particular to a method for manufacturing an amorphous motor iron core. Background Art
[0002] With the increasing prominence of energy issues and the continuous improvement of environmental protection awareness, motors, as one of the main energy-consuming devices, have higher and higher requirements for energy-saving and environmental protection performance. Traditional motor core materials can no longer meet the high efficiency, energy-saving and environmental protection requirements of modern motors due to problems such as insufficient magnetic properties, large losses and heavy weight. Therefore, the development of a new motor core material and its manufacturing method is of great significance to improving motor performance, reducing energy consumption and promoting the sustainable development of the motor industry.
[0003] As a new type of material with excellent magnetic properties and low loss characteristics, amorphous alloy has broad application prospects in the field of motor core manufacturing. However, the manufacturing and processing of amorphous alloys are difficult, especially in terms of raw material ratio, molding process and heat treatment process, which require fine control to ensure the performance and stability of the core. Therefore, the present invention proposes a method for manufacturing an amorphous motor core, which aims to achieve efficient and low-loss manufacturing of an amorphous motor core by optimizing the raw material ratio, molding process and heat treatment process. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for manufacturing an amorphous motor core, which achieves efficient and low-loss manufacturing of the amorphous motor core by finely controlling the raw material ratio and optimizing the molding process and the heat treatment process.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for manufacturing an amorphous motor core, the specific method is as follows:
[0006] Step S1, raw material processing process, processing the raw materials and accurately proportioning them, the raw materials mainly consist of iron, silicon, boron and carbon;
[0007] Step S2, forming process, based on step S2, forming operation is performed on the proportioned raw materials, and the forming process mainly includes melting, rapid cooling, crushing, pre-pressing, fine pressing, set and shaping steps;
[0008] Step S3, heat treatment process, based on step S3, the formed iron core blank is treated, and the heat treatment process includes annealing, crystallization treatment, tempering, magnetic field treatment and surface strengthening treatment;
[0009] Step S4, a post-processing process, is to post-process the formed iron core based on step S3, and the post-processing process includes measurement, detection and recycling.
[0010] Preferably, the specific ratio range of iron, silicon, boron and carbon in the raw materials is as follows:
[0011] The iron content is 75%-85%, the silicon content is 10%-18%, the boron content is 3%-7%, and the carbon content is 0.5%-2%.
[0012] Preferably, the raw material processing includes screening and cleaning.
[0013] Preferably, the precise proportioning of raw materials is as follows:
[0014] High-precision measuring equipment is used to measure the raw materials precisely, and the content of each element is accurate to two decimal places.
[0015] Preferably, the molding process is specifically performed as follows:
[0016] Melting stage: melt the proportioned raw materials at high temperature to form a uniform melt, and the melting temperature is controlled between 1450℃-1550℃;
[0017] Rapid cooling stage: The melt is quickly cooled to room temperature to form an amorphous thin strip or powder to form an amorphous material;
[0018] Crushing stage: the cooled amorphous material is crushed into fine particles, which are then screened and cleaned;
[0019] Pre-pressing stage: Use a primary pressing mold to preliminarily press the crushed amorphous particles to form a preliminary iron core shape;
[0020] Fine pressing stage: Use high-precision pressing equipment and technology to further finely press the initially pressed iron chips;
[0021] Assembly stage: The finely pressed iron core sheets are assembled according to the design requirements to form a complete amorphous motor core;
[0022] Shaping stage: The assembled core is shaped, including grinding and polishing steps.
[0023] Preferably, during the smelting stage, the proportioned raw materials are melted in an inert atmosphere.
[0024] Preferably, the heat treatment process is specifically performed as follows:
[0025] Annealing stage: Place the pressed iron core in an annealing furnace and perform annealing at a temperature of 500℃-600℃;
[0026] Crystallization treatment stage: Control the heating speed and holding time to partially crystallize the amorphous structure in the core and form a microstructure that is beneficial to improving magnetic properties;
[0027] Tempering stage: secondary heating and heat preservation of the iron core;
[0028] Magnetic field treatment stage: During the heating, insulation and cooling process, a longitudinal magnetic field is applied to the core;
[0029] In the surface strengthening treatment stage, ion nitriding, laser cladding and physical vapor deposition methods are used to strengthen the surface of the amorphous motor core.
[0030] Preferably, the post-processing process is specifically performed as follows:
[0031] Measuring stage: According to the size standard, use a high-precision electronic measuring ruler to measure the iron core;
[0032] Testing stage: testing the surface and magnetic force of the core;
[0033] Recycling stage: The substandard formed cores are recycled for secondary processing.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. The present invention manufactures an amorphous motor core in sequence through a raw material processing process, a molding process, a heat treatment process and a post-processing process, wherein the raw materials are processed and accurately proportioned, and then formed through smelting, rapid cooling, crushing, pre-pressing, fine pressing, fitting and shaping steps, and then the manufacturing is completed through a heat treatment process including annealing, crystallization treatment, tempering, magnetic field treatment and surface strengthening treatment, and finally measurement and testing are performed to ensure the accuracy of the core. By optimizing the raw material ratio, improving the molding process and heat treatment technology, efficient and low-loss manufacturing of amorphous motor cores is achieved.
[0036] 2. When the raw materials are smelted, the present invention places the raw materials in an inert atmosphere and uses inert gas protection during the smelting process to prevent oxidation of the raw materials.
[0037] 3. The present invention removes impurities and oxides in the raw materials by screening and cleaning the raw materials, thereby avoiding adverse effects on the properties of the alloy.
[0038] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The present invention is a flow chart of the method for manufacturing an amorphous motor core;
[0040] Figure 2It is a schematic diagram of a flow chart of the raw material processing process of the present invention;
[0041] Figure 3 is a flow chart of the molding process of the present invention;
[0042] Figure 4 is a flow chart of the heat treatment process of the present invention;
[0043] Figure 5 It is a flow chart of the post-processing process of the present invention. DETAILED DESCRIPTION
[0044] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this technical field without creative work are within the scope of protection of the present invention.
[0045] Please refer to the figure, a method for manufacturing an amorphous motor core, the specific method is as follows:
[0046] Step S1, raw material processing process, processing the raw materials and accurately proportioning them, the raw materials mainly consist of iron, silicon, boron and carbon;
[0047] Step S2, forming process, based on step S2, forming operation is performed on the proportioned raw materials, and the forming process mainly includes melting, rapid cooling, crushing, pre-pressing, fine pressing, set and shaping steps;
[0048] Step S3, heat treatment process, based on step S3, the formed iron core blank is treated, and the heat treatment process includes annealing, crystallization treatment, tempering, magnetic field treatment and surface strengthening treatment;
[0049] Step S4, a post-processing process, is to post-process the formed iron core based on step S3, and the post-processing process includes measurement, detection and recycling.
[0050] Specifically, the manufacturing method of the amorphous motor core in the present invention is similar to the existing manufacturing method of the amorphous motor core. The main improvement of the present invention is that by finely controlling the raw material ratio, optimizing the molding process and the heat treatment process, the efficient and low-loss manufacturing of the amorphous motor core is realized; the present invention sequentially manufactures the motor core through the raw material processing process, the molding process, the heat treatment process and the post-processing process, wherein the raw materials are selected to be composed of iron, silicon, boron and carbon. According to the different use scenarios and performance requirements of the core, other alloy elements such as tungsten, molybdenum, chromium, etc. can also be added in appropriate amounts to further improve the amorphous alloy. The properties of gold are determined by processing the raw materials and then accurately proportioning them. By accurately controlling the content of each element, it can be ensured that the amorphous alloy has excellent magnetic and mechanical properties and the accuracy of the raw material proportion is guaranteed. It is then formed through smelting, rapid cooling, crushing, pre-pressing, fine pressing, fitting and shaping steps, and then manufactured through heat treatment processes including annealing, crystallization treatment, tempering, magnetic field treatment and surface strengthening treatment. Finally, measurement and testing are carried out to ensure the accuracy of the core. By optimizing the raw material proportion, improving the forming process and heat treatment technology, efficient and low-loss manufacturing of amorphous motor cores is achieved.
[0051] Specifically, the specific ratio ranges of iron, silicon, boron and carbon in the raw materials are as follows:
[0052] The iron content is 75%-85%, the silicon content is 10%-18%, the boron content is 3%-7%, and the carbon content is 0.5%-2%; according to the different usage scenarios and performance requirements of the iron core, the percentage of iron, silicon, boron and carbon is adjusted appropriately within the content range, and the content of each element is accurately controlled to ensure the performance of the amorphous alloy.
[0053] Specifically, the raw material processing methods include screening and cleaning; removing impurities and oxides in the raw materials to avoid adverse effects on the alloy properties and ensure the performance of the amorphous motor core.
[0054] Specifically, the precise proportioning of raw materials is as follows:
[0055] High-precision metering equipment is used to measure the raw materials precisely, and the content of each element is accurate to two decimal places; high-precision metering equipment is used to measure the raw materials of each element, which improves the accuracy of the ratio of the content of each element, thereby ensuring quality and facilitating mass production.
[0056] Specifically, the molding process is performed as follows:
[0057] Melting stage: melt the proportioned raw materials at high temperature to form a uniform melt. The melting temperature is controlled between 1450℃-1550℃ to ensure that the raw materials are fully melted and mixed evenly.
[0058] Rapid cooling stage: The melt is quickly cooled to room temperature to form an amorphous thin strip or powder, forming an amorphous material; the cooling speed is controlled, and the cooling process parameters are optimized to ensure the formation of an amorphous state and avoid the occurrence of crystallization;
[0059] Crushing stage: the cooled amorphous material is crushed into fine particles, which are then screened and cleaned. The size and shape of the particles are controlled during the crushing process to meet the requirements of the subsequent pressing process and ensure the uniformity and purity of the particles.
[0060] Pre-pressing stage: Use primary pressing molds to preliminarily press the crushed amorphous particles to form a preliminary iron core sheet shape; control the pressure and temperature during the pre-pressing process to ensure the basic shape and structure of the iron core sheet is stable;
[0061] Fine pressing stage: Use high-precision pressing equipment and technology to further finely press the preliminarily pressed iron core pieces; by precisely controlling parameters such as pressure, temperature and time, the high density and excellent performance of the iron core pieces can be achieved;
[0062] Assembly stage: The finely pressed iron core sheets are assembled according to the design requirements to form a complete amorphous motor core. During the assembly process, the overlap size between each group of iron core sheets must be accurate to ensure the stability and reliability of the motor operation.
[0063] Shaping stage: The assembled core is shaped, including grinding and polishing steps; through grinding and polishing, the surface defects of the amorphous motor core are eliminated and the appearance quality of the core is improved. During the shaping process, the shaping force and speed are controlled to avoid damage to the internal structure of the core.
[0064] Specifically, during the smelting stage, the proportioned raw materials are melted in an inert atmosphere; inert gas protection is used during the smelting process to prevent oxidation of the raw materials and ensure the formation of an amorphous state.
[0065] Specifically, the heat treatment process is performed as follows:
[0066] Annealing stage: Place the pressed core in an annealing furnace and perform heat preservation annealing at 500℃-600℃ to eliminate the internal stress of the core and improve the magnetic properties. The annealing temperature and time are precisely controlled according to the composition and size of the core.
[0067] Crystallization treatment stage: Control the heating rate and holding time to partially crystallize the amorphous structure in the core and form a microstructure that is beneficial to improving the magnetic properties; strictly control the heating rate and holding time during the crystallization treatment to avoid excessive crystallization leading to performance degradation.
[0068] Tempering stage: the iron core is heated and kept warm again to further improve its stability and corrosion resistance. The tempering temperature and time are precisely controlled according to the performance requirements of the iron core.
[0069] Magnetic field treatment stage: During the heating, insulation and cooling process, a longitudinal magnetic field is applied to the iron core; magnetic field treatment can further improve the magnetic and mechanical properties of the iron core and improve the operating efficiency of the motor. The magnetic field intensity and treatment time are adjusted according to the specific requirements of the iron core;
[0070] In the surface strengthening treatment stage, the surface of the amorphous motor core is strengthened by ion nitriding, laser cladding and physical vapor deposition. The surface of the amorphous motor core is treated by one or more of the methods of ion nitriding, laser cladding and physical vapor deposition. These technologies can significantly improve the hardness, wear resistance and corrosion resistance of the core surface, thereby enhancing the overall performance and service life of the core.
[0071] Specifically, the post-processing process is performed as follows:
[0072] Measuring stage: According to the size standard, use a high-precision electronic measuring ruler to measure the iron core; perform high-precision multi-directional measurement on the formed iron core to confirm that the size meets the standard;
[0073] Inspection stage: inspect the surface and magnetism of the core; use equipment to inspect the surface and magnetism of the core to ensure that there are no defects on the core surface and that the magnetism of the core meets the standard;
[0074] Recycling and processing stage: The formed iron cores that do not meet the standards are recycled for secondary processing; when the size, surface flatness and magnetic force of the core do not meet the standards, the core will be recycled and processed twice to reduce waste and avoid the outflow of defective products.
[0075] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for manufacturing an amorphous motor core, characterized in that: The specific method is as follows: Step S1, raw material processing process, processing the raw materials and accurately proportioning them, the raw materials mainly consist of iron, silicon, boron and carbon; Step S2, forming process, based on step S2, forming operation is performed on the proportioned raw materials, and the forming process mainly includes melting, rapid cooling, crushing, pre-pressing, fine pressing, set and shaping steps; Step S3, heat treatment process, based on step S3, the formed iron core blank is treated, and the heat treatment process includes annealing, crystallization treatment, tempering, magnetic field treatment and surface strengthening treatment; Step S4, a post-processing process, is to post-process the formed iron core based on step S3, and the post-processing process includes measurement, detection and recycling.
2. The method for manufacturing an amorphous motor core according to claim 1, characterized in that: The specific ratio ranges of iron, silicon, boron and carbon in the raw materials are as follows: The iron content is 75%-85%, the silicon content is 10%-18%, the boron content is 3%-7%, and the carbon content is 0.5%-2%.
3. The method for manufacturing an amorphous motor core according to claim 1, characterized in that: Raw material processing includes screening and cleaning.
4. The method for manufacturing an amorphous motor core according to claim 1, characterized in that: The precise proportion of raw materials is as follows: High-precision measuring equipment is used to measure the raw materials precisely, and the content of each element is accurate to two decimal places.
5. The method for manufacturing an amorphous motor core according to claim 1, characterized in that: The specific operation of the molding process is as follows: Melting stage: melt the proportioned raw materials at high temperature to form a uniform melt, and the melting temperature is controlled between 1450℃-1550℃; Rapid cooling stage: The melt is quickly cooled to room temperature to form an amorphous thin strip or powder to form an amorphous material; Crushing stage: the cooled amorphous material is crushed into fine particles, which are then screened and cleaned; Pre-pressing stage: Use a primary pressing mold to preliminarily press the crushed amorphous particles to form a preliminary iron core shape; Fine pressing stage: Use high-precision pressing equipment and technology to further finely press the initially pressed iron chips; Assembly stage: The finely pressed iron core sheets are assembled according to the design requirements to form a complete amorphous motor core; Shaping stage: The assembled core is shaped, including grinding and polishing steps.
6. The method for manufacturing an amorphous motor core according to claim 5, characterized in that: During the smelting stage, the proportioned raw materials are melted in an inert atmosphere.
7. The method for manufacturing an amorphous motor core according to claim 5, characterized in that: The heat treatment process is as follows: Annealing stage: Place the pressed iron core in an annealing furnace and perform annealing at a temperature of 500℃-600℃; Crystallization treatment stage: Control the heating speed and holding time to partially crystallize the amorphous structure in the core and form a microstructure that is beneficial to improving magnetic properties; Tempering stage: secondary heating and heat preservation of the iron core; Magnetic field treatment stage: During the heating, insulation and cooling process, a longitudinal magnetic field is applied to the core; In the surface strengthening treatment stage, ion nitriding, laser cladding and physical vapor deposition methods are used to strengthen the surface of the amorphous motor core.
8. The method for manufacturing an amorphous motor core according to claim 6, characterized in that: The specific operation of post-processing process is as follows: Measuring stage: According to the size standard, use a high-precision electronic measuring ruler to measure the iron core; Testing stage: testing the surface and magnetic force of the core; Recycling stage: The substandard formed cores are recycled for secondary processing.